Solar cell, preparation method thereof and solar cell polishing solution
By forming a specific tower base texture structure and a pyramid texture structure on the second and third surfaces of the solar cell, the impact of tower base morphology and size on performance is solved, and the short-circuit current and fill factor of the solar cell are improved. The open circuit voltage is maintained and the overall efficiency is improved.
Patent Information
- Application Number
- CN202410670836.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2024-09-24
AI Technical Summary
The morphology, structure and size of the tower base in existing solar cells have an impact on performance, resulting in a decrease in efficiency, and it is difficult to further improve the overall efficiency while keeping the size of the tower base unchanged.
By forming a specific tower base suede structure on the second and third surfaces of the solar cell, including dispersedly arranged depressions and pyramid structures, and processing with polishing fluid, the depth and specific surface area of the depressions are controlled to improve contact area and flatness.
The contact area between the slurry and the tower base is increased, the short-circuit current and filling factor are increased, while the open-circuit voltage remains unchanged, and the overall efficiency of the solar cell is improved.
Smart Images

Figure CN118693176A
Abstract
Description
Technical Field
[0001] The present application relates to the field of photovoltaic technology, and in particular to a solar cell and a preparation method thereof, and a solar cell polishing liquid. Background Art
[0002] In order to cope with the global energy shortage and the increasing depletion of traditional energy (fossil, coal, oil, etc.), it has become a consensus to vigorously develop renewable energy. Solar energy has become one of the fastest-growing renewable energy sources due to its significant advantages such as cleanliness, safety, and abundant resources, and photovoltaic power generation is one of the most important ways to use solar energy.
[0003] At present, most solar cells use a velvet structure on the back of the tower base. Now all research subjects use a structure with a reduced size of the back tower base. However, in practical applications, the morphology, structure and size of the tower base will also affect the performance of the solar cell. Summary of the invention
[0004] Based on this, it is necessary to provide a solar cell and a preparation method thereof and a solar cell polishing liquid to improve the morphology of the tower base, minimize the influence of the morphology, structure and size of the tower base on the performance of the solar cell, and improve the overall efficiency of the solar cell.
[0005] In a first aspect, a solar cell is provided, the solar cell comprising:
[0006] A substrate, the substrate having a first surface and a second surface arranged opposite to each other along a thickness direction thereof; wherein the first surface has a first pyramid velvet structure, and the second surface has a first tower base velvet structure;
[0007] The first tower base velvet surface structure includes a first reference plane, and a plurality of dispersedly arranged depressions formed on the first reference plane, each depression constitutes a tower base, and an area on the first reference plane where no depression is formed forms a top surface of a plurality of tower bases;
[0008] Among them, the side length of each tower base is 6μm~8μm, the side surface of each depression has a rounded transition with the bottom surface of the depression and the top surface of the tower base corresponding to the depression, and the depth of each depression is less than or equal to 300nm, and the specific surface area of the velvet structure of the first tower base is 1.16~1.25, or, the depth of each depression is greater than or equal to 800nm, and the specific surface area of the velvet structure of the first tower base is 1.2~2.
[0009] Optionally, the depth of each of the depressions is greater than 0 nm and less than or equal to 300 nm, or the depth of each of the depressions is 800 nm to 2 μm.
[0010] Optionally, the depth of each of the depressions is greater than or equal to 800 nm, and the angle between the side surface of each of the depressions and the bottom surface of the depression is 110° to 130°; or,
[0011] The depth of each of the depressions is less than or equal to 300 nm, and the angle between the side surface of each of the depressions and the bottom surface of the depression is 130° to 150°.
[0012] Optionally, the first pyramid velvet structure includes a plurality of pyramid structures and a plurality of notches formed on the side of each pyramid structure, and each of the notches is formed by a plurality of hole structures arranged around the side of the pyramid structure.
[0013] Optionally, the specific surface area of the first pyramid velvet structure is 1.4~3.
[0014] Optionally, the side length of the base of each pyramid structure is 1 μm to 3 μm.
[0015] Optionally, the height of each of the pyramid structures is 0.5 μm to 3 μm.
[0016] In a second aspect, a solar cell polishing liquid is provided, the polishing liquid comprising: a polishing liquid base component, and an auxiliary polishing agent;
[0017] Wherein, the auxiliary polishing agent includes potassium hydroxyethylidene diphosphate and diethylenetriamine pentaacetic acid, and the mass ratio of the potassium hydroxyethylidene diphosphate to the diethylenetriamine pentaacetic acid is 0.3~0.5, or the mass ratio of the potassium hydroxyethylidene diphosphate to the diethylenetriamine pentaacetic acid is 0.15~0.25.
[0018] In a third aspect, a method for preparing a solar cell is provided, comprising:
[0019] Providing a substrate, the substrate having a first surface and a second surface disposed opposite to each other along a thickness direction thereof, and a third surface adjacent to the first surface and the second surface;
[0020] Performing texturing and element doping treatment on the first surface of the substrate to form a first pyramid texture structure and a silicon doped layer on the first surface, wherein the first pyramid texture structure and the silicon doped layer also extend to cover the second surface and the third surface;
[0021] The second surface and the third surface are polished by using the polishing liquid as described in the second aspect, so as to form a first tower base velvet structure on the second surface and the third surface;
[0022] The first tower base velvet structure includes a first reference plane, and a plurality of recesses dispersedly arranged on the first reference plane, each recess constituting a tower base, and an area on the first reference plane where no recess is formed forms a plurality of top surfaces of the tower bases; wherein a side length of each tower base is 6μm~8μm, a rounded transition is formed between the side surface of each recess and the bottom surface of the recess and the top surface of the tower base corresponding to the recess, and a depth of each recess is less than or equal to 300nm, and a specific surface area of the first tower base velvet structure is 1.16~1.25, or a depth of each recess is greater than or equal to 800nm, and a specific surface area of the first tower base velvet structure is 1.2~2.
[0023] Optionally, the polishing treatment is performed at a temperature of 50° C. to 70° C. and for a time of 100 s to 200 s.
[0024] Optionally, texturing the first surface of the substrate comprises:
[0025] The substrate is etched by using a first texturing agent to form a second pyramid textured surface structure on the first surface, the second surface and the third surface of the substrate, wherein the second pyramid textured surface structure comprises: a plurality of pyramid structures;
[0026] The substrate is etched again with a second texturing agent to form a plurality of notches on the side of each pyramid structure, thereby forming the first pyramid texture surface structure; wherein each of the notches is formed by a plurality of hole structures arranged around the side of the pyramid structure.
[0027] Optionally, the first texturing agent comprises: a texturing agent base component;
[0028] The second texturing agent comprises: a texturing agent base component and an auxiliary etching agent;
[0029] The auxiliary etching agent includes: polyether compound and sodium lignin sulfonate.
[0030] Optionally, the auxiliary etchant accounts for 0.1 wt% to 0.2 wt% of the second texturing agent.
[0031] Optionally, the temperature of the second etching is 50° C. to 80° C., and the time is 50s to 100s.
[0032] In a fourth aspect, a solar cell is provided, comprising:
[0033] A substrate having a first surface and a second surface disposed opposite to each other along a thickness direction of the substrate;
[0034] Among them, the first surface has a first pyramid velvet structure, and the second surface has a second pyramid base velvet structure; the first pyramid velvet structure includes a plurality of pyramid structures, and a plurality of notches formed on the side of each pyramid structure, and each of the notches is formed by a plurality of hole structures arranged around the side of the pyramid structure.
[0035] In a fifth aspect, a method for preparing a solar cell is provided, comprising:
[0036] Providing a substrate, the substrate having a first surface and a second surface disposed opposite to each other along a thickness direction thereof, and a third surface adjacent to the first surface and the second surface;
[0037] Performing texturing and element doping treatment on the first surface of the substrate to form a first pyramid texture structure and a silicon doped layer on the first surface, wherein the first pyramid texture structure and the silicon doped layer also extend to cover the second surface and the third surface; and
[0038] The second surface and the third surface are polished by a polishing liquid to form a second tower base velvet structure on the second surface and the third surface;
[0039] The first surface of the substrate is textured, comprising:
[0040] The substrate is etched by using a first texturing agent to form a second pyramid textured surface structure on the first surface, the second surface and the third surface of the substrate, wherein the second pyramid textured surface structure comprises: a plurality of pyramid structures;
[0041] The substrate is etched again with a second texturing agent to form a plurality of notches on the side of each pyramid structure to form the first pyramid texture structure; wherein each of the notches is formed by a plurality of hole structures arranged around the side of the pyramid structure.
[0042] Optionally, before the second surface and the third surface are polished with a polishing liquid and the second suede structure is formed on the second surface and the third surface, the preparation method further comprises:
[0043] The second surface and the third surface formed with the first textured structure are textured again to remove the silicon doped layer plated on the second surface and the third surface.
[0044] Compared with the related art, the beneficial technical effects of this application are as follows:
[0045] For the size of each tower base of 6μm~8μm, by controlling the depth of each depression to be deeper, compared with the depth of each depression of 500nm in the related art, the specific surface area of the tower base can be further increased, thereby increasing the contact area between the slurry and the tower base, and further improving the short-circuit current and fill factor of the solar cell. Since the side surface of each depression and the bottom surface of the depression and the top surface of the tower base corresponding to the depression are rounded, and when the depth of each depression is greater than or equal to 800nm, the specific surface area of the velvet structure of the first tower base is 1.16~1.25, therefore, the specific surface area of the velvet structure of the first tower base is relatively small, and the surface roughness is small, which is reflected in the morphology that the velvet structure of the first tower base is relatively smooth and has fewer burrs, so that the solar cell can be maintained. The open-circuit voltage of the cell remains basically unchanged, thereby improving the overall efficiency of the solar cell; by controlling the depth of each depression to be shallower, compared with the depth of each depression of 500nm in the related art, the specific surface area of the tower base can be reduced and the flatness of the tower base can be improved, and by controlling the specific surface area of the velvet structure of the first tower base to be 1.2~2, the surface roughness of the velvet structure of the first tower base can also be kept small, that is, reflected in the morphology that the velvet structure of the first tower base also has fewer burrs, thereby improving the passivation performance of the solar cell, thereby improving the open-circuit voltage of the solar cell, and at the same time, since the size of the tower base remains unchanged, it is found through testing that the shallower depth of the tower base does not bring about a large loss of fill factor, and can also improve the overall efficiency of the solar cell.
[0046] In summary, the present application can further improve the overall efficiency of the solar cell while keeping the size of the tower base unchanged. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.
[0048] Figure 1 A schematic cross-sectional structure diagram of a substrate provided in an embodiment of the present application;
[0049] Figure 2 A scanning electron microscope image of a second surface of a substrate provided in an embodiment of the present application;
[0050] Figure 3 A scanning electron microscope image of the second surface of another substrate provided in an embodiment of the present application;
[0051] Figure 4A schematic structural diagram of a depression in a tower base provided in an embodiment of the present application;
[0052] Figure 5 A scanning electron microscope image of a first surface of a substrate provided in an embodiment of the present application;
[0053] Figure 6 A schematic diagram of a process for preparing a solar cell provided in an embodiment of the present application;
[0054] Figure 7 A schematic flow chart of another method for preparing a solar cell provided in an embodiment of the present application. DETAILED DESCRIPTION
[0055] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0056] Unless the context requires otherwise, throughout the specification and claims, the term "including" is to be interpreted as an open, inclusive meaning, that is, "including, but not limited to". In the description of the specification, the terms "one embodiment", "some embodiments", "exemplary embodiments", "exemplarily" or "some examples" and the like are intended to indicate that specific features, structures, materials or characteristics associated with the embodiment or example are included in at least one embodiment or example of the present disclosure. The schematic representation of the above terms does not necessarily refer to the same embodiment or example. In addition, the specific features, structures, materials or characteristics may be included in any one or more embodiments or examples in any appropriate manner.
[0057] Exemplary embodiments are described herein with reference to cross-sectional views and / or plan views that are idealized exemplary drawings. In the drawings, the thickness of layers and regions are exaggerated for clarity. Therefore, variations in shape relative to the drawings due to, for example, manufacturing techniques and / or tolerances are conceivable. Therefore, the exemplary embodiments should not be interpreted as being limited to the shapes of the regions shown herein, but include shape deviations due to, for example, manufacturing. For example, an etched region shown as a rectangle will typically have curved features. Therefore, the regions shown in the drawings are schematic in nature, and their shapes are not intended to illustrate the actual shape of regions of the device, and are not intended to limit the scope of the exemplary embodiments.
[0058] Herein, unless otherwise specified, "one or more" means one or more than or equal to two.
[0059] In this document, "for example", "such as", "example", "for example", etc. are used for descriptive purposes, indicating that the previous and subsequent different technical solutions are related in terms of the content covered, but should not be understood as limiting the previous technical solution, nor can they be understood as limiting the scope of protection of this document. In this document, unless otherwise specified, A (such as B) means that B is a non-limiting example of A, and it can be understood that A is not limited to B.
[0060] In this document, the terms "first", "second", etc. in "the first aspect", "the second aspect", etc. are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features.
[0061] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0062] In this article, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0063] Herein, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values within the numerical interval is considered to be continuous and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when a numerical interval only refers to integers within the numerical interval, including the two endpoint integers of the numerical range, and each integer between the two endpoints, is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical ranges disclosed herein should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows broadly including numerical interval types such as percentage intervals, ratio intervals, and ratio intervals.
[0064] In this article, when it comes to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.
[0065] As used in this article, fill factor (FF) refers to the ratio of the actual maximum achievable power (Pm or Vmp * Jmp) to the theoretical (not actually achievable) power (Jsc * Voc). Therefore, FF can be determined by the following formula:
[0066] FF = (Vmp * Jmp) / (Jsc * Voc)
[0067] Where Jmp and Vmp represent the current density and voltage at the maximum power point (Pm), which is obtained by changing the resistance in the circuit until J * V is the maximum value; Jsc and Voc represent the short-circuit current and open-circuit voltage, respectively. Fill factor is a key parameter for evaluating solar cells. Commercial solar cells usually have a fill factor of about 60% or more.
[0068] As used herein, open circuit voltage (Voc) is the potential difference between the anode and cathode of the device with no external load connected.
[0069] The power conversion efficiency (PCE) of a solar cell used in this article refers to the percentage of power converted from absorbed light to electrical energy. The power conversion efficiency (PCE) of a solar cell can be measured by the incident light irradiance (E: W / m 2 ) and the surface area of the solar cell (Ac:m 2 ) divided by the maximum power point (Pm). STC usually refers to the temperature of 25℃ and the irradiance of 1000 W / m 2 , the spectrum of air quality 1.5 (AM1.5).
[0070] Since parameters such as the morphology, structure and size of the tower base will affect the performance of solar cells, for example, as the size of the tower base in related technologies becomes smaller and smaller, the specific surface area of the tower base can be increased to a certain extent, thereby increasing the contact between the tower base and the slurry, improving the contact performance of the solar cell, and then improving the fill factor of the solar cell; however, how to further improve the overall efficiency of the solar cell while keeping the size of the tower base unchanged is still a goal that people are constantly pursuing.
[0071] In a first aspect, some embodiments of the present application provide a solar cell, which includes: a substrate, and other functional layers disposed on the substrate, such as a tunneling oxide layer, a passivation layer, and an electrode pattern.
[0072] Here, taking the solar cell as a TOPCon (Tunnel Oxide Passivated Contact) solar cell as an example, the solar cell includes: a substrate, a first passivation layer and a first electrode pattern arranged on the front side of the substrate, and a tunneling oxide layer, an N-type doped polysilicon layer, a second passivation layer and a second electrode pattern arranged on the back side of the substrate.
[0073] In some embodiments, Figure 1As shown, the substrate 1 has a first surface 11 and a second surface 12 arranged opposite to each other along the thickness direction thereof; wherein the first surface 11 has a first pyramid velvet structure, and the second surface 12 has a first tower base velvet structure. The first surface 11 can be the front side of the substrate 1, and the second surface 12 can be the back side of the substrate 1.
[0074] In some embodiments, Figure 1 , Figure 2 , Figure 3 and Figure 4 As shown, the first tower base velvet structure includes a first reference plane M, and a plurality of recesses U dispersedly arranged on the first reference plane M, each recess U constitutes a tower base 121, and the area on the first reference plane M where the recess U is not formed forms the top surfaces a of the plurality of tower bases 121; wherein the side length r of each tower base 121 is 6 μm to 8 μm, and a rounded transition is formed between the side surface b of each recess U and the bottom surface c of the recess U and the top surface a of the tower base 121 corresponding to the recess U, and, as shown Figure 1 and Figure 2 As shown, the depth t of each depression U is less than or equal to 300 nm, and the specific surface area of the first tower base velvet structure is 1.16 to 1.25, or, as Figure 1 and Figure 3 As shown, the depth t of each depression U is greater than or equal to 800 nm, and the specific surface area of the velvet structure of the first tower base is 1.2~2.
[0075] The side length r of each tower base 121 is 6 μm to 8 μm, which means that the side lengths r of each tower base can be the same or different and are independently 6 μm to 8 μm. Here, it can also be regarded that the size of each tower base 121 is 6 μm to 8 μm.
[0076] That is, in the embodiment of the present application, when the size of the tower base 121 remains unchanged, the depth t of each recess U can be adjusted to be shallower or deeper compared with the related art.
[0077] Here, the specific surface area of the first tower base velvet structure refers to the ratio of the surface area of the first tower base velvet structure to the surface area of the second surface which is a smooth surface (which can be regarded as a plane of the first tower base velvet structure without forming uneven surfaces), which can be used to characterize the roughness of the first tower base velvet structure.
[0078] In the solar cell provided in the embodiment of the present application, for the size of each tower base 121 being 6 μm to 8 μm, Figure 1 and Figure 3As shown in FIG. 1 , by controlling the depth t of each depression U to be deeper, compared with the depth of each depression of 500 nm in the related art, the specific surface area of the tower base can be further increased, thereby increasing the contact area between the slurry and the tower base, thereby further improving the short-circuit current and fill factor of the solar cell. Figure 1 and Figure 4 As shown, since there is a rounded transition between the side surface b of each depression U and the bottom surface c of the depression U and the top surface a of the tower base 121 corresponding to the depression, and when the depth of each depression U is greater than or equal to 800nm, the specific surface area of the first tower base velvet structure is 1.16~1.25, therefore, the specific surface area of the first tower base velvet structure is relatively small, and the surface roughness is small, which is reflected in the morphology that the first tower base velvet structure is relatively smooth and has fewer burrs, so that the open circuit voltage of the solar cell can be kept basically unchanged, thereby improving the overall efficiency of the solar cell; and as shown in FIG. Figure 1 and Figure 2 As shown, by controlling the depth t of each depression U to be shallower, compared with the depth of each depression of 500nm in the related art, the specific surface area of the tower base can be reduced and the flatness of the tower base can be improved. By controlling the specific surface area of the first tower base velvet structure to be 1.2~2, the surface roughness of the first tower base velvet structure can also be maintained at a smaller surface, that is, it is reflected in the morphology that the first tower base velvet structure also has fewer burrs, thereby improving the passivation performance of the solar cell, and then improving the open circuit voltage of the solar cell. At the same time, since the size of the tower base 121 remains unchanged, it is found through testing that the shallower depth of the tower base 121 does not result in a large loss of fill factor, and can also improve the overall efficiency of the solar cell.
[0079] In summary, the present application can further improve the overall efficiency of the solar cell while keeping the size of the tower base unchanged.
[0080] In some embodiments, the depth t of each recess U is greater than 0 nm and less than or equal to 300 nm, or the depth t of each recess U is 800 nm to 2 μm.
[0081] In these embodiments, by controlling the depth t of the recess U to be greater than 0 nm and less than or equal to 300 nm, or the depth of the recess U to be within the range of 800 nm to 2 μm, it can be ensured that the solar cell has a higher overall efficiency.
[0082] Here, it should be noted that, since the side surface b of the concave U and the bottom surface c of the concave U and the top surface a of the tower base 121 corresponding to the concave U are rounded transitions, the angle θ between the side surface b of the concave U and the bottom surface c of the concave U can be the tangent line between the side surface b of the concave U and the bottom surface c of the concave U (such as Figure 4 The angle between the dashed lines shown.
[0083] In some embodiments, Figure 3 and Figure 4 As shown, when the depth t of each concavity U is greater than or equal to 800 nm, the angle θ between the side surface b of each concavity U and the bottom surface c of the concavity U is 110°~130°.
[0084] In these embodiments, by limiting the angle θ between the side surface b of each recess U and the bottom surface c of the recess U to within the range of 110° to 130°, the recess U can be made relatively flat, and the open circuit voltage can be kept substantially unchanged as much as possible while maintaining a high fill factor of the solar cell, thereby improving the overall efficiency of the solar cell.
[0085] In some embodiments, Figure 2 and Figure 4 As shown, when the depth t of each concave U is less than or equal to 300 nm, the angle θ between the side surface b of each concave U and the bottom surface c of the concave U is 130°~150°.
[0086] In these embodiments, by limiting the angle θ between the side surface b of each recess U and the bottom surface c of the recess U to within the range of 130° to 150°, the recess U can be made flatter, thereby further improving the passivation performance without causing significant damage to the fill factor, thereby further improving the overall efficiency of the solar cell.
[0087] The first pyramid velvet structure may include a plurality of pyramid structures. In this case, the specific surface area of the first pyramid velvet structure may be greater than or equal to 1.1, for example, the specific surface area of the first pyramid velvet structure may be 1.33.
[0088] The specific surface area here refers to the ratio of the surface area of the first pyramid velvet structure to the surface area of the first smooth surface (which can be regarded as a plane without forming the uneven first pyramid velvet structure), which can be used to characterize the roughness of the first pyramid velvet structure.
[0089] In some embodiments, Figure 5 As shown, the first pyramid velvet structure includes a plurality of pyramid structures 111 and a plurality of notches g formed on the side of each pyramid structure 111 , and each notch g is formed by a plurality of hole structures arranged around the side of the pyramid structure 111 .
[0090] In these embodiments, by setting a plurality of notches g on the side of each pyramid structure 111, each notch g is formed by a plurality of hole structures arranged around the side of the pyramid structure 111, so that the plurality of notches g can increase the specific surface area and roughness of the first surface 11 to a certain extent, on the one hand, this greatly increases the light trapping efficiency, making the short-wave effect of the solar cell more excellent; on the other hand, it can reduce the reflectivity of the first pyramid velvet structure to a certain extent; on the other hand, it can increase the contact area between the first surface and the slurry, reduce the contact resistance, and thus further improve the filling factor of the solar cell. At the same time, since each notch g is formed by a plurality of hole structures arranged around the side of the pyramid structure 111, the first pyramid velvet structure can be kept with a relatively small specific surface area, so that the degradation of the passivation performance caused by excessive specific surface area can be avoided while maintaining the high filling factor of the solar cell, and the overall efficiency of the solar cell can be further improved.
[0091] In some embodiments, the specific surface area of the first pyramid velvet structure is 1.4-3.
[0092] Here, the specific surface area of the first pyramid velvet structure refers to the ratio of the surface area of the first pyramid velvet structure to the surface area of the first surface which is a smooth surface (which can be regarded as a plane of the first pyramid velvet structure without uneven surfaces), which can be used to characterize the roughness of the first pyramid velvet structure.
[0093] In these embodiments, by controlling the specific surface area of the first pyramid velvet structure within the range of 1.4 to 3, the contact area between the first surface and the slurry can be increased, and the contact resistance can be reduced, thereby further improving the fill factor of the solar cell and avoiding a decrease in passivation performance due to excessive roughness, thereby improving the overall efficiency of the solar cell.
[0094] For example, the specific surface area of the first pyramid velvet structure may be 1.48 to 1.57.
[0095] In some embodiments, there is a distance between two adjacent notches, and the distance is 0.1 μm-0.9 μm.
[0096] In some embodiments, Figure 1 and Figure 5 As shown, the side length p of the base of each pyramid structure 111 is 1 μm to 3 μm.
[0097] In these embodiments, the side length p (ie, size) of the base of each pyramid structure 111 is relatively small, which can give the first surface a relatively large specific surface area and roughness, thereby improving the light trapping effect.
[0098] In some embodiments, Figure 1 and Figure 5 As shown, the height h of each pyramid structure 111 is 0.5 μm to 3 μm.
[0099] In these embodiments, the height h of each pyramid structure 111 is in the range of 0.5 μm to 3 μm, which can give the first surface a relatively large specific surface area and roughness, thereby improving the light trapping effect.
[0100] In a second aspect, some embodiments of the present application provide a solar cell polishing liquid, the polishing liquid comprising: a polishing liquid base component, and an auxiliary polishing agent;
[0101] The auxiliary polishing agent comprises potassium hydroxyethylidene diphosphate and diethylenetriamine pentaacetic acid, and the mass ratio of potassium hydroxyethylidene diphosphate to diethylenetriamine pentaacetic acid is 0.3-0.5, or the mass ratio of potassium hydroxyethylidene diphosphate to diethylenetriamine pentaacetic acid is 0.15-0.25.
[0102] Wherein, the polishing liquid matrix component can be any polishing liquid purchased by commercial means that can polish the substrate of the solar cell. By adding an auxiliary polishing agent to the polishing liquid and adjusting the mass ratio of hydroxyethylidene diphosphate potassium and the diethylenetriamine pentaacetic acid in the auxiliary polishing agent to 0.3-0.5, the depth of each depression can be controlled to be less than or equal to 300nm while keeping the size of the tower base unchanged, thereby reducing the specific surface area and roughness of the second surface, making the second surface flat, and then improving the passivation performance and the open circuit voltage of the solar cell. In the whole process, the size of the tower base can remain unchanged, so that the fill factor loss can be not caused while increasing the open circuit voltage of the solar cell. By adjusting the mass ratio of potassium hydroxyethylidene diphosphate and the diethylenetriamine pentaacetic acid in the auxiliary polishing agent to 0.15-0.25, the depth of each depression can be controlled to be greater than or equal to 800nm while the size of the tower base remains basically unchanged, and the specific surface area of the tower base can be increased to above 1.2, so that the contact area between the tower base and the slurry is further increased, thereby improving the filling factor of the solar cell. At the same time, it is found through testing that the overall efficiency of the solar cell obtained in this way is also greatly improved.
[0103] In some embodiments, when the mass ratio of potassium hydroxyethylidene diphosphate to diethylenetriaminepentaacetic acid is 0.3-0.5, the mass proportion of potassium hydroxyethylidene diphosphate in the polishing liquid is 0.5%-1.0%, and the mass proportion of diethylenetriaminepentaacetic acid in the polishing liquid is 1.0%-1.5%.
[0104] In these embodiments, by controlling the mass proportions of potassium hydroxyethylidene diphosphate and diethylenetriamine pentaacetic acid in the polishing liquid within the above ranges, a tower base with a recessed depth less than or equal to 300 nm can be obtained, thereby reducing the specific surface area and roughness of the second surface, making the second surface smooth, thereby improving the passivation performance and increasing the open circuit voltage of the solar cell.
[0105] In some embodiments, when the mass ratio of potassium hydroxyethylidene diphosphate to diethylenetriaminepentaacetic acid is 0.15-0.25, the mass proportion of potassium hydroxyethylidene diphosphate in the polishing liquid is 0.15%-0.25%, and the mass proportion of diethylenetriaminepentaacetic acid in the polishing liquid is 1.0%-1.5%.
[0106] In these embodiments, by controlling the mass proportions of potassium hydroxyethylidene diphosphate and diethylenetriamine pentaacetic acid in the polishing liquid within the above-mentioned ranges, a tower base with a recessed depth greater than or equal to 800 nm can be obtained, thereby increasing the specific surface area and roughness of the second surface, increasing the fill factor of the solar cell, and thereby increasing the overall efficiency of the solar cell.
[0107] In some embodiments, the polishing liquid matrix components may include: sodium persulfate, sodium iodate, sodium gluconate, an acidic compound, and an alkaline compound.
[0108] Among them, in the polishing liquid, the mass proportion of sodium persulfate is 1.5%~2.5%, the mass proportion of sodium iodate is 2.5%~4.0%, the mass proportion of sodium gluconate is 1.0%~1.5%, the mass proportion of acidic compounds is 0.75%~1.45%, and the mass proportion of alkaline compounds is 0.4%~0.7%.
[0109] In some embodiments, the acidic compound may include at least one of phosphoric acid, sulfuric acid, and acetic acid.
[0110] In some examples, the acidic compound includes phosphoric acid, sulfuric acid and acetic acid, and the mass proportion of phosphoric acid in the polishing liquid is 0.1%~0.25%, the mass proportion of sulfuric acid in the polishing liquid is 0.45%~0.65%, and the mass proportion of acetic acid in the polishing liquid is 0.3%~0.6%.
[0111] In some embodiments, the phosphoric acid can be selected from concentrated phosphoric acid having a concentration greater than or equal to 85%, and the sulfuric acid can be selected from concentrated sulfuric acid having a concentration greater than or equal to 98%.
[0112] Concentrated phosphoric acid, concentrated sulfuric acid and acetic acid may be mixed in proportion to obtain an acidic solution, and the polishing liquid may be prepared by mixing the acidic solution with other components and water.
[0113] In some embodiments, the alkaline compound may include at least one of potassium hydroxide and sodium hydroxide.
[0114] In some examples, the alkaline compound may include potassium hydroxide and / or sodium hydroxide, and in the case where the alkaline compound may include potassium hydroxide and sodium hydroxide, the mass proportion of potassium hydroxide in the polishing liquid is 0.2%~0.3%, and the mass proportion of sodium hydroxide in the polishing liquid is 0.2%~0.4%.
[0115] In some embodiments, potassium hydroxide and sodium hydroxide may be separately prepared into solutions, and then the prepared solutions are mixed according to a proportion, and then mixed with other components and water in a proportion to prepare the polishing liquid.
[0116] In a third aspect, some embodiments of the present application provide a method for preparing a solar cell, such as Figure 6 As shown, the preparation method includes the following steps S61), S62) and S63).
[0117] S61), providing a substrate, the substrate having a first surface and a second surface arranged opposite to each other along a thickness direction thereof, and a third surface adjacent to the first surface and the second surface;
[0118] The first surface and the second surface may be the front and back sides of the substrate, and the third surface may be the side surface of the substrate.
[0119] S62), performing texturing and element doping treatment on the first surface of the substrate to form a first pyramid texture structure and a silicon doped layer on the first surface, wherein the first pyramid texture structure and the silicon doped layer also extend to cover the second surface and the third surface;
[0120] The element doping treatment here may be a P-type doping element doping treatment or an N-type doping element doping treatment. For example, taking the solar cell as an N-type TOPCon solar cell, the element may be a P-type doping element, such as element B.
[0121] When the first surface of the substrate is textured and doped with elements, wraparound expansion is also formed on the second surface and the third surface, thereby forming a first pyramid texture structure and a silicon doping layer on the second surface and the third surface.
[0122] The silicon doped layer may be formed in the first pyramid texture structure and have a certain thickness.
[0123] S63), polishing the second surface and the third surface with the polishing liquid as described in the second aspect, to form a first tower base suede structure on the second surface and the third surface;
[0124] The tower base velvet structure includes a first reference plane, and a plurality of dispersedly arranged depressions formed on the first reference plane, each depression constitutes a tower base, and the area on the first reference plane where no depressions are formed forms the top surfaces of a plurality of tower bases; wherein the side length of each tower base is 6μm~8μm, the side surface of each depression and the bottom surface of the depression and the top surface of the tower base corresponding to the depression have a rounded transition, and the depth of each depression is less than or equal to 300nm, and the specific surface area of the first tower base velvet structure is 1.16~1.25, or the depth of each depression is greater than or equal to 800nm, and the specific surface area of the first tower base velvet structure is 1.2~2.
[0125] In step S63), by polishing the first pyramid velvet structure on the second surface and the third surface, the first pyramid velvet structure and the silicon doping layer can be removed, and the second surface and the third surface can be processed into the first pyramid base velvet structure.
[0126] In the method for preparing a solar cell provided in an embodiment of the present application, the second surface and the third surface are polished by using the polishing liquid as described in the second aspect. Since potassium hydroxyethylidene diphosphate and diethylenetriaminepentaacetic acid are added to the polishing liquid, on the one hand, the corrosion rate of the substrate in different crystal directions can be controlled. Experiments have shown that when the mass ratio of potassium hydroxyethylidene diphosphate and diethylenetriaminepentaacetic acid is 0.3~0.5, the depth of each depression can be controlled to be less than or equal to 300nm. The second surface thus obtained is relatively flat, which can effectively improve the passivation performance of the solar cell, thereby increasing the open circuit voltage of the solar cell; and when the mass ratio of potassium hydroxyethylidene diphosphate to diethylenetriamine pentaacetic acid is 0.15-0.25, the depth of each depression can be controlled to be greater than or equal to 800nm while keeping the size of the tower base unchanged, so that the depth of the depression can be increased to a certain extent while keeping the second surface relatively smooth and having fewer burrs, which is convenient for increasing the contact area between the second surface and the slurry and reducing the contact resistance, thereby increasing the short-circuit current and fill factor of the solar cell while keeping the open circuit voltage slightly changed, thereby improving the overall efficiency of the solar cell.
[0127] In some embodiments, the polishing process is performed at a temperature of 50° C. to 70° C. and for a time of 100 s to 200 s.
[0128] In some embodiments, texturing the first surface of the substrate may include:
[0129] The substrate is etched by using a first texturing agent to form a second pyramid textured surface structure on the first surface, the second surface and the third surface of the substrate, wherein the second pyramid textured surface structure comprises: a plurality of pyramid structures;
[0130] The substrate is etched again with a second texturing agent to modify the surface of each pyramid structure, forming a plurality of notches on the side of each pyramid structure to form a first pyramid velvet structure; wherein each notch is formed by a plurality of hole structures arranged around the side of the pyramid structure.
[0131] In these embodiments, after preparing a plurality of pyramid structures, a second texturing agent is used to etch the surfaces of the plurality of pyramid structures again, so that a plurality of notches can be formed on the side of each pyramid structure, and each notch is formed by a plurality of hole structures arranged around the side of the pyramid structure. This can increase the roughness of the first surface to a certain extent, thereby further improving the light trapping effect and open circuit voltage of the solar cell. At the same time, it can also avoid excessive roughness, thereby reducing the open circuit voltage loss caused by poor passivation effect.
[0132] In some embodiments, the first texturing agent includes: a texturing agent base component;
[0133] The second texturing agent includes: a texturing agent base component and an auxiliary etching agent;
[0134] The auxiliary etching agents include: polyether compounds and sodium lignin sulfonate.
[0135] In these embodiments, by adding polyether compounds and sodium lignin sulfonate, the polyether compounds and sodium lignin sulfonate can be used to selectively corrode the side of the pyramid structure during etching again, thereby forming a plurality of scratches formed by a plurality of hole structures arranged around the side of the pyramid structure as above, thereby avoiding adverse effects caused by excessive roughness while ensuring a certain roughness.
[0136] In some embodiments, the auxiliary etchant accounts for 0.1% to 0.2% by mass in the second texturing agent.
[0137] In these embodiments, the mass proportion of the auxiliary etchant in the second texturing agent is within the above range, and the specific surface area of the first surface can be adjusted to 1.4~3, thereby reducing the open circuit voltage loss caused by the reduction of passivation performance while increasing the surface roughness.
[0138] In some embodiments, the temperature of the second etching is 50° C. to 80° C., and the time is 50 s to 100 s.
[0139] In some embodiments, the texturing agent base component included in the first texturing agent and the texturing agent base component included in the second texturing agent may be the same or different, which is not specifically limited herein.
[0140] In some embodiments, taking the case where the first and second texturing agents contain the same texturing agent base component, the first and second texturing agents contain the same texturing agent base component, which may include: 2-methyl-2,4-pentanediol, sodium carboxymethyl cellulose, 5-nitroguaiacol, 5-chloro-2-(2',4'-dichlorophenoxy)phenol, sodium hydroxide, sodium acetate, sodium chloride, and pigments, etc. Among them, the pigments may include: one or more of beetroot red, erythrosine, caramel II, and nobiletin.
[0141] Among them, in the first texturing agent, the mass proportion of 2-methyl-2,4-pentanediol is 0.2%~0.3%, the mass proportion of sodium carboxymethyl cellulose is 1.5%~2.0%, the mass proportion of 5-nitroguaiacol is 0.18%~0.22%, the mass proportion of 5-chloro-2-(2',4'-dichlorophenoxy)phenol is 0.2%~0.25%, the mass proportion of sodium hydroxide is 0.3%~0.5%; the mass proportion of sodium acetate is 0.15%~0.25%; the mass proportion of sodium chloride is 0.2%~0.4%.
[0142] In the second texturing agent, the mass proportion of 2-methyl-2,4-pentanediol is 0.2%~0.3%, the mass proportion of sodium carboxymethyl cellulose is 1.5%~2.0%, the mass proportion of 5-nitroguaiacol is 0.18%~0.22%, the mass proportion of 5-chloro-2-(2',4'-dichlorophenoxy)phenol is 0.2%~0.25%, the mass proportion of sodium hydroxide is 0.3%~0.5%; the mass proportion of sodium acetate is 0.15%~0.25%; the mass proportion of sodium chloride is 0.2%~0.4%, the mass proportion of polyether compounds is 0.05%~0.1%, and the mass proportion of sodium lignin sulfonate is 0.05%~0.1%.
[0143] In these embodiments, the selective corrosion described above can be achieved by controlling the mass ratio of the polyether compound to the sodium lignin sulfonate within the above range, thereby forming a plurality of notches on the side of each pyramid structure.
[0144] In some embodiments, the polyether compound may include one or more of fatty alcohol polyoxyethylene ether, octylphenol polyoxyethylene ether, propylene glycol block polyether and polyoxyethylene polyoxypropylene ether.
[0145] In a fourth aspect, some embodiments of the present application provide a solar cell, such as Figure 1 and Figure 5 As shown, the solar cell comprises:
[0146] A substrate 1, wherein the substrate 1 has a first surface 11 and a second surface 12 arranged opposite to each other along a thickness direction thereof;
[0147] Among them, the first surface 11 has a first pyramid velvet structure, and the second surface 12 has a second pyramid base velvet structure. The first pyramid velvet structure includes a plurality of pyramid structures 111, and a plurality of notches g formed on the side of each pyramid structure 111, and each notch g is formed by a plurality of hole structures arranged around the side of the pyramid structure 111.
[0148] In some embodiments, the specific surface area of the first pyramid velvet structure is 1.4-3.
[0149] In some embodiments, there is a distance between two adjacent notches g, and the distance is 0.1 μm-0.9 μm.
[0150] In some embodiments, the side length p of the base of each pyramid structure 111 is 1 μm-3 μm.
[0151] In these embodiments, the side length p (ie, size) of the base of each pyramid structure 111 is relatively small, which can give the first surface a larger specific surface area and roughness, thereby improving the light trapping effect.
[0152] In some embodiments, the height h of each pyramid structure 111 is 0.5 μm-3 μm.
[0153] In these embodiments, the height h of each pyramid structure 111 is in the range of 0.5 μm to 3 μm, which can give the first surface a larger specific surface area and roughness, thereby improving the light trapping effect.
[0154] In a fifth aspect, some embodiments of the present application provide a method for preparing a solar cell, such as Figure 7 As shown, the preparation method comprises:
[0155] S71), providing a substrate, wherein the substrate has a first surface and a second surface arranged opposite to each other along a thickness direction thereof, and a third surface adjacent to the first surface and the second surface;
[0156] The first surface and the second surface may be the front and back sides of the substrate, and the third surface may be the side surface of the substrate.
[0157] S72), performing texturing and element doping treatment on the first surface of the substrate to form a first pyramid texture structure and a silicon doped layer on the first surface, wherein the first pyramid texture structure and the silicon doped layer also extend to cover the second surface and the third surface; and
[0158] S73), polishing the second surface and the third surface with a polishing liquid to form a second tower base suede structure on the second surface and the third surface;
[0159] Wherein, S72), texturing the first surface of the substrate comprises:
[0160] S721), etching the substrate with a first texturing agent to form a second pyramid texture structure on the first surface, the second surface and the third surface of the substrate, wherein the second pyramid texture structure includes: a plurality of pyramid structures;
[0161] S722), using a second texturing agent to etch the substrate again, forming a plurality of grooves on the side of each pyramid structure to form a first pyramid velvet structure; wherein each groove is formed by a plurality of hole structures arranged around the side of the pyramid structure.
[0162] In these embodiments, multiple grooves are formed on the side of each pyramid structure through secondary texturing. Since each groove is composed of multiple hole structures arranged around the side of the pyramid structure, compared with the relatively smooth surface of each pyramid structure in the related art, the roughness of the first surface can be increased to a certain extent, thereby further improving the light trapping effect and open circuit voltage of the solar cell. At the same time, it can also avoid excessive roughness, thereby reducing the open circuit voltage loss caused by poor passivation effect.
[0163] In some embodiments, the first texturing agent includes: a texturing agent base component;
[0164] The second texturing agent includes: a texturing agent base component and an auxiliary etching agent;
[0165] The auxiliary etching agents include: polyether compounds and sodium lignin sulfonate.
[0166] In these embodiments, by adding polyether compounds and sodium lignin sulfonate, the polyether compounds and sodium lignin sulfonate can be used to selectively corrode the side of the pyramid structure during etching again, thereby forming a plurality of scratches formed by a plurality of hole structures arranged around the side of the pyramid structure as above, thereby avoiding adverse effects caused by excessive roughness while ensuring a certain roughness.
[0167] In some embodiments, the auxiliary etchant accounts for 0.1 wt% to 0.2 wt% of the second texturing agent.
[0168] In these embodiments, the mass proportion of the auxiliary etchant in the second texturing agent is within the above range, and the specific surface area of the first surface can be adjusted to 1.4~3, thereby reducing the open circuit voltage loss caused by the reduction of passivation performance while increasing the surface roughness.
[0169] In some embodiments, the temperature of the second etching is 50° C. to 80° C., and the time is 50 s to 100 s.
[0170] In some embodiments, the texturing agent base component included in the first texturing agent and the texturing agent base component included in the second texturing agent may be the same or different, which is not specifically limited herein.
[0171] In some embodiments, taking the case where the first and second texturing agents contain the same texturing agent base component, the first and second texturing agents contain the same texturing agent base component, which may include: 2-methyl-2,4-pentanediol, sodium carboxymethyl cellulose, 5-nitroguaiacol, 5-chloro-2-(2',4'-dichlorophenoxy)phenol, sodium hydroxide, sodium acetate, sodium chloride, and pigments, etc. Among them, the pigments may include: one or more of beetroot red, erythrosine, caramel II, and nobiletin.
[0172] Among them, in the first texturing agent, the mass proportion of 2-methyl-2,4-pentanediol is 0.2%~0.3%, the mass proportion of sodium carboxymethyl cellulose is 1.5%~2.0%, the mass proportion of 5-nitroguaiacol is 0.18%~0.22%, the mass proportion of 5-chloro-2-(2',4'-dichlorophenoxy)phenol is 0.2%~0.25%, the mass proportion of sodium hydroxide is 0.3%~0.5%; the mass proportion of sodium acetate is 0.15%~0.25%; the mass proportion of sodium chloride is 0.2%~0.4%.
[0173] In the second texturing agent, the mass proportion of 2-methyl-2,4-pentanediol is 0.2%~0.3%, the mass proportion of sodium carboxymethyl cellulose is 1.5%~2.0%, the mass proportion of 5-nitroguaiacol is 0.18%~0.22%, the mass proportion of 5-chloro-2-(2',4'-dichlorophenoxy)phenol is 0.2%~0.25%, the mass proportion of sodium hydroxide is 0.3%~0.5%; the mass proportion of sodium acetate is 0.15%~0.25%; the mass proportion of sodium chloride is 0.2%~0.4%, the mass proportion of polyether compounds is 0.05%~0.1%, and the mass proportion of sodium lignin sulfonate is 0.05%~0.1%.
[0174] In some embodiments, the polyether compound may include one or more of fatty alcohol polyoxyethylene ether, octylphenol polyoxyethylene ether, propylene glycol block polyether and polyoxyethylene polyoxypropylene ether.
[0175] In some embodiments, in S73), the second surface and the third surface are polished with a polishing liquid, and before the second tower base velvet structure is formed on the second surface and the third surface, the preparation method further includes:
[0176] The second surface and the third surface formed with the first textured structure are textured again to remove the silicon doping layer plated on the second surface and the third surface.
[0177] In these embodiments, before the second surface and the third surface are polished, the second surface and the third surface formed with the first pyramid velvet structure and the silicon-doped layer are subjected to a second texturing treatment, so that the silicon-doped layer plated on the second surface and the third surface can be removed by etching with a texturing liquid, thereby reducing the silicon-doped layer residue on the second surface and the third surface and reducing the leakage on the side. At the same time, the second texturing can also increase the etching depth, so as to facilitate the subsequent polishing process to obtain a smaller-sized tower base.
[0178] For example, the size of the tower base of the second tower base texture structure may be 2 μm to 4 μm.
[0179] In order to objectively evaluate the technical effects of the embodiments of the present application, the present application will be described in detail and exemplarily through the following embodiments and comparative examples.
[0180] In the following examples and comparative examples, all raw materials can be purchased commercially, and in order to maintain the reliability of the experiment, the raw materials used in the following examples and comparative examples have the same physical and chemical parameters or are prepared by the same processing method.
[0181] Example 1
[0182] The method for preparing the solar cell provided in Example 1 is as follows:
[0183] S10), the front side of the N-type silicon wafer is textured and doped with B element to form a second pyramid texture structure and a PN junction; wherein the second pyramid texture structure includes: a plurality of pyramid structures, and the texture agent used for the texture includes: 0.25wt% of 2-methyl-2,4-pentanediol, 1.8wt% of sodium carboxymethyl cellulose, 0.2wt% of 5-nitroguaiacol, 0.22wt% of triclosan, 0.4wt% of sodium hydroxide, 0.2wt% of sodium acetate, 0.3wt% of sodium chloride, 0.05wt% of pigment and water.
[0184] S20), polishing the back and side of the N-type silicon wafer at 60°C for 150s, forming a first tower base velvet structure on the back and side of the N-type silicon wafer, wherein the size of the tower base in the tower base velvet structure is 7μm, and the height of the tower base (i.e., the depth of the depression in the tower base) is 300nm. The composition of the polishing liquid used for the polishing treatment is shown in Table 1 below, and the mass proportion of hydroxyethylidene diphosphoric acid is 0.5%, and the mass proportion of diethylenetriamine pentaacetic acid is 1.5%.
[0185] Table 1
[0186]
[0187] S30), forming a tunneling oxide layer and an N-type doped polysilicon layer on the back side of the N-type silicon wafer;
[0188] S40), forming passivation layers on the front and back sides of the N-type silicon wafer obtained in S30), and sintering to prepare gate line patterns.
[0189] Example 2
[0190] The method for preparing the solar cell in Example 2 is substantially the same as the method for preparing the solar cell in Example 1, except that:
[0191] In step S20), the height of the tower base is 100 nm; in the polishing liquid, the mass proportion of hydroxyethylidene diphosphonic acid is 0.5%, and the mass proportion of diethylenetriamine pentaacetic acid is 1.0%.
[0192] Example 3
[0193] The method for preparing the solar cell in Example 3 is substantially the same as the method for preparing the solar cell in Example 1, except that:
[0194] In step S20), the height of the tower base is 200 nm; in the polishing liquid, the mass proportion of hydroxyethylidene diphosphonic acid is 0.4%, and the mass proportion of diethylenetriamine pentaacetic acid is 1.0%.
[0195] Example 4
[0196] The method for preparing the solar cell in Example 4 is substantially the same as the method for preparing the solar cell in Example 1, except that:
[0197] In step S20), the height of the tower base is 800 nm; in the polishing liquid, the mass proportion of hydroxyethylidene diphosphonic acid is 0.15%, and the mass proportion of diethylenetriamine pentaacetic acid is 1.0%.
[0198] Example 5
[0199] The method for preparing the solar cell in Example 5 is substantially the same as the method for preparing the solar cell in Example 1, except that:
[0200] In step S20), the height of the tower base is 900 nm; in the polishing liquid, the mass proportion of hydroxyethylidene diphosphonic acid is 0.25%, and the mass proportion of diethylenetriamine pentaacetic acid is 1.0%.
[0201] Example 6
[0202] The method for preparing the solar cell in Example 6 is substantially the same as the method for preparing the solar cell in Example 1, except that:
[0203] In step S20), the height of the tower base is 1000 nm; in the polishing liquid, the mass proportion of hydroxyethylidene diphosphonic acid is 0.25%, and the mass proportion of diethylenetriamine pentaacetic acid is 1.5%.
[0204] Comparative Example 1
[0205] The method for preparing the solar cell in Comparative Example 1 is substantially the same as the method for preparing the solar cell in Example 1, except that:
[0206] In step S20), the height of the tower base is 500 nm; and the polishing liquid does not contain hydroxyethylidene diphosphonic acid and diethylenetriamine pentaacetic acid.
[0207] Example 7
[0208] The method for preparing the solar cell in Example 7 is substantially the same as the method for preparing the solar cell in Example 1, except that:
[0209] In step S10), the front side of the N-type silicon wafer is textured twice, and the textured agent used in the first textured process is the same as the textured agent used in Example 1, and the textured agent used in the second textured process also includes: 0.08wt% of a polyether compound and 0.08wt% of sodium lignin sulfonate, to obtain a first pyramid textured surface structure. In addition to a plurality of pyramid structures, the first pyramid textured surface structure also includes a plurality of notches formed on the side of each pyramid structure, and each notch is formed by a plurality of hole structures arranged around the side of the pyramid structure.
[0210] Example 8
[0211] The method for preparing the solar cell in Example 8 is substantially the same as the method for preparing the solar cell in Example 7, except that:
[0212] The texturing agent used in the second texturing also includes: 0.05wt% of polyether compound and 0.1wt% of sodium lignin sulfonate.
[0213] Example 9
[0214] The method for preparing the solar cell in Example 9 is substantially the same as the method for preparing the solar cell in Example 7, except that:
[0215] The texturing agent used in the second texturing also includes: 0.1wt% of polyether compound and 0.05wt% of sodium lignin sulfonate.
[0216] Example 10
[0217] The method for preparing the solar cell in Example 10 is substantially the same as the method for preparing the solar cell in Example 1, except that:
[0218] In step S10), the front side of the N-type silicon wafer is textured for the second time. The textured agent used in the first texture is the same as the textured agent used in Example 1. The textured agent used in the second texture also includes: 0.08wt% of a polyether compound and 0.08wt% of sodium lignin sulfonate, to obtain a first pyramid velvet structure. In addition to a plurality of pyramid structures, the first pyramid velvet structure also includes a plurality of notches formed on the side of each pyramid structure, and each notch is formed by a plurality of hole structures arranged around the side of the pyramid structure.
[0219] In step S20), the height of the tower base is 500 nm; and the polishing liquid does not contain hydroxyethylidene diphosphonic acid and diethylenetriamine pentaacetic acid.
[0220] Embodiment 11
[0221] The method for preparing the solar cell in Example 11 is substantially the same as the method for preparing the solar cell in Example 10, except that:
[0222] Before step S20), the method further includes: performing a second texturing treatment on the second surface and the third surface formed with the first pyramid texture structure to remove the B-doped silicon layer plated on the second surface and the third surface. The composition of the texturing agent used in the second texturing treatment is the same as the composition of the texturing agent used in step S10 in embodiment 1.
[0223] Example 12
[0224] The method for preparing the solar cell in Example 12 is substantially the same as the method for preparing the solar cell in Example 10, except that:
[0225] In step S10), the texturing agent used in the second texturing further includes: 0.05 wt % of a polyether compound and 0.1 wt % of sodium lignin sulfonate.
[0226] Embodiment 13
[0227] The method for preparing the solar cell in Example 13 is substantially the same as the method for preparing the solar cell in Example 10, except that:
[0228] In step S10), the texturing agent used in the second texturing further includes: 0.1 wt % of a polyether compound and 0.05 wt % of sodium lignin sulfonate.
[0229] Test Case
[0230] 1. The specific surface area and reflectivity of the front pyramid velvet structure of the N-type silicon wafer provided in Examples 1 to 13 and Comparative Example 1 and the specific surface area of the back tower base velvet structure were tested, and the test results are shown in Table 2 below:
[0231] Table 2
[0232]
[0233] Among them, in Table 2, the specific surface area testing method of the front pyramid velvet structure and the back tower base velvet structure is: Examples 1 to 13 and Comparative Example 1 both use 1000 N-type silicon wafers for experiments, use ZETA20-3D to output the specific surface area under a 100x optical microscope, and take the average value in each example and comparative example to obtain the result; the reflectivity testing method of the front pyramid velvet structure is: Examples 1 to 13 and Comparative Example 1 both use 1000 N-type silicon wafers for experiments, use D8 reflectivity tester to test the reflectivity of the front pyramid velvet structure, and take the average value in each example and comparative example to obtain the result.
[0234] It can be seen from Table 2 that the specific surface area and reflectivity of the front pyramid velvet structure of the silicon wafers of Examples 1 to 6 provided in the present application are basically unchanged or slightly changed compared with Comparative Example 1, while the specific surface area and reflectivity of the front pyramid velvet structure of the silicon wafers of Examples 7 to 13 are greatly changed compared with Comparative Example 1, which means that by preparing the first pyramid velvet structure on the front side of the silicon wafer, the specific surface area and reflectivity of the front pyramid velvet structure can be increased to a certain extent; and the specific surface area of the back tower base velvet structure of the silicon wafers of Examples 1 to 3 and 7 to 9 provided in the embodiments of the present application is greatly changed compared with Comparative Example 1, while the specific surface area of the back tower base velvet structure of the silicon wafers of Examples 4 to 6, and Example 10, and Example 12 to 13 is not much changed compared with Comparative Example 1, and the back tower base velvet structure of the silicon wafers of Examples 4 to 6 can be kept with fewer burrs, and because the tower base size is smaller in Example 11, the specific surface area of the back tower base velvet structure of the silicon wafer is further increased relative to Example 10.
[0235] 2. The short-circuit current, open-circuit voltage, fill factor, etc. of 1000 solar cells provided in Examples 1 to 13 and Comparative Example 1 were tested and averaged respectively, and the photoelectric conversion efficiency of the solar cells in Examples 1 to 13 and Comparative Example 1 was calculated. The specific test and calculation results are shown in Table 3 below:
[0236] Table 3
[0237]
[0238] It can be seen from Table 3 that the open circuit voltage of the solar cells of Examples 1 to 3, Examples 7 to 9, Example 10, and Examples 12 to 13 provided by the present application is greatly improved compared with Comparative Example 1, while the short-circuit current and fill factor of the solar cells of Examples 1 to 3 are basically unchanged or slightly changed compared with Comparative Example 1, which indicates that when the depression of the tower base of the embodiments of the present application becomes shallower, the open circuit voltage of the solar cell can be increased while keeping the short-circuit current and fill factor basically unchanged, thereby improving the efficiency of the solar cell to a certain extent; and the short-circuit current and fill factor of the solar cells of Examples 4 to 6, Examples 7 to 9, and Examples 10 to 13 are greatly improved compared with Comparative Example 1, which indicates that the depression of the tower base of the embodiments of the present application is shallower. When the depression becomes deeper, or the specific surface area of the tower base is slightly increased, and the specific surface area of the front pyramid velvet structure is slightly increased, the short-circuit current and the fill factor of the solar cell can be increased while the open-circuit voltage is kept basically unchanged, thereby improving the efficiency of the solar cell to a certain extent; the open-circuit voltage of the solar cells of Examples 7 to 9, as well as Examples 10 and Examples 12 to 13 changes little, because the specific surface area of the velvet structure of the back tower base of Examples 7 to 9, as well as Examples 10 and Examples 12 to 13 changes little, and basically does not have a significant impact on the open-circuit voltage; and the open-circuit voltage of the solar cell of Example 11 changes greatly relative to that of Example 10, because the tower base size of the velvet structure of the back tower base of Example 11 becomes smaller.
[0239] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0240] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A solar cell, characterized in that: The solar cell comprises: A substrate, the substrate having a first surface and a second surface arranged opposite to each other along a thickness direction thereof; wherein the first surface has a first pyramid suede structure, and the second surface has a first tower base suede structure; The first tower base velvet surface structure includes a first reference plane, and a plurality of dispersedly arranged depressions formed on the first reference plane, each depression constitutes a tower base, and an area on the first reference plane where no depression is formed forms a top surface of a plurality of tower bases; Among them, the side length of each tower base is 6μm~8μm, the side surface of each depression has a rounded transition with the bottom surface of the depression and the top surface of the tower base corresponding to the depression, and the depth of each depression is less than or equal to 300nm, and the specific surface area of the velvet structure of the first tower base is 1.16~1.25, or, the depth of each depression is greater than or equal to 800nm, and the specific surface area of the velvet structure of the first tower base is 1.2~2.
2. The solar cell according to claim 1, characterized in that: The depth of each of the depressions is greater than 0 nm and less than or equal to 300 nm, or the depth of each of the depressions is 800 nm to 2 μm.
3. The solar cell according to claim 1, characterized in that The depth of each of the depressions is greater than or equal to 800 nm, and the angle between the side surface of each of the depressions and the bottom surface of the depression is 110° to 130°; or, The depth of each of the depressions is less than or equal to 300 nm, and the angle between the side surface of each of the depressions and the bottom surface of the depression is 130° to 150°.
4. The solar cell according to any one of claims 1 to 3, characterized in that: The first pyramid velvet structure includes a plurality of pyramid structures and a plurality of notches formed on the side of each pyramid structure, and each of the notches is formed by a plurality of hole structures arranged around the side of the pyramid structure.
5. The solar cell according to claim 4, characterized in that: The specific surface area of the first pyramid velvet structure is 1.4~3.
6. The solar cell according to claim 4, characterized in that: The side length of the base of each pyramid structure is 1 μm to 3 μm.
7. The solar cell according to claim 4, characterized in that: The height of each pyramid structure is 0.5 μm to 3 μm.
8. A solar cell polishing liquid, characterized in that: The polishing liquid comprises: a polishing liquid base component and an auxiliary polishing agent; Wherein, the auxiliary polishing agent includes potassium hydroxyethylidene diphosphate and diethylenetriamine pentaacetic acid, and the mass ratio of the potassium hydroxyethylidene diphosphate to the diethylenetriamine pentaacetic acid is 0.3~0.5, or the mass ratio of the potassium hydroxyethylidene diphosphate to the diethylenetriamine pentaacetic acid is 0.15~0.
25.
9. A method for preparing a solar cell, characterized in that: include: Providing a substrate, the substrate having a first surface and a second surface disposed opposite to each other along a thickness direction thereof, and a third surface adjacent to the first surface and the second surface; Performing texturing and element doping treatment on the first surface of the substrate to form a first pyramid texture structure and a silicon doped layer on the first surface, wherein the first pyramid texture structure and the silicon doped layer also extend to cover the second surface and the third surface; The second surface and the third surface are polished by the polishing liquid as claimed in claim 8 to form a first tower base velvet structure on the second surface and the third surface; The first tower base velvet structure includes a first reference plane, and a plurality of recesses dispersedly arranged on the first reference plane, each recess constituting a tower base, and an area on the first reference plane where no recess is formed forms a plurality of top surfaces of the tower bases; wherein a side length of each tower base is 6μm~8μm, a rounded transition is formed between the side surface of each recess and the bottom surface of the recess and the top surface of the tower base corresponding to the recess, and a depth of each recess is less than or equal to 300nm, and a specific surface area of the first tower base velvet structure is 1.16~1.25, or a depth of each recess is greater than or equal to 800nm, and a specific surface area of the first tower base velvet structure is 1.2~2.
10. The preparation method according to claim 9, characterized in that: The polishing process is performed at a temperature of 50° C. to 70° C. and for a time of 100 s to 200 s.
11. The preparation method according to claim 9, characterized in that: Texturing the first surface of the substrate comprises: The substrate is etched by using a first texturing agent to form a second pyramid textured surface structure on the first surface, the second surface and the third surface of the substrate, wherein the second pyramid textured surface structure comprises: a plurality of pyramid structures; The substrate is etched again with a second texturing agent to form a plurality of notches on the side of each pyramid structure, thereby forming the first pyramid texture surface structure; wherein each of the notches is formed by a plurality of hole structures arranged around the side of the pyramid structure.
12. The preparation method according to claim 11, characterized in that: The first texturing agent comprises: a texturing agent base component; The second texturing agent comprises: a texturing agent base component and an auxiliary etching agent; The auxiliary etching agent includes: polyether compound and sodium lignin sulfonate.
13. The preparation method according to claim 12, characterized in that: The auxiliary etchant accounts for 0.1 wt% to 0.2 wt% of the second texturing agent.
14. The preparation method according to any one of claims 11 to 13, characterized in that: The temperature of the second etching is 50° C. to 80° C., and the time is 50s to 100s.
15. A solar cell, characterized in that: The solar cell comprises: A substrate having a first surface and a second surface disposed opposite to each other along a thickness direction of the substrate; Among them, the first surface has a first pyramid velvet structure, and the second surface has a second pyramid base velvet structure; the first pyramid velvet structure includes a plurality of pyramid structures, and a plurality of notches formed on the side of each pyramid structure, and each of the notches is formed by a plurality of hole structures arranged around the side of the pyramid structure.
16. A method for preparing a solar cell, characterized in that: include: Providing a substrate, the substrate having a first surface and a second surface disposed opposite to each other along a thickness direction thereof, and a third surface adjacent to the first surface and the second surface; Performing texturing and element doping treatment on the first surface of the substrate to form a first pyramid texture structure and a silicon doped layer on the first surface, wherein the first pyramid texture structure and the silicon doped layer also extend to cover the second surface and the third surface; as well as The second surface and the third surface are polished by using a polishing liquid to form a second tower base velvet surface structure on the second surface and the third surface; The first surface of the substrate is textured, comprising: The substrate is etched by using a first texturing agent to form a second pyramid textured surface structure on the first surface, the second surface and the third surface of the substrate, wherein the second pyramid textured surface structure comprises: a plurality of pyramid structures; The substrate is etched again with a second texturing agent to form a plurality of notches on the side of each pyramid structure to form the first pyramid texture structure; wherein each of the notches is formed by a plurality of hole structures arranged around the side of the pyramid structure.
17. The preparation method according to claim 16, characterized in that: Before the second surface and the third surface are polished by a polishing liquid and a second tower base velvet structure is formed on the second surface and the third surface, the preparation method further comprises: The second surface and the third surface are subjected to texturing treatment again to remove the silicon doping layer plated around the second surface and the third surface.
Citation Information
Cited By
Solar cell silicon wafer and preparation method thereof
CN118610285A
Silicon wafer for solar cell and its preparation method
CN118610285B
Back contact battery with multi-layer gradient textured structure and manufacturing method and application thereof
CN119451314A
A back contact battery with a multi-layer gradient suede structure and its preparation method and application
CN119451314B