Control method giving consideration to wire rod bearing steel hot rolling structure and network carbide
Through the four-stage air-cooling cooling mode, carbide precipitation is controlled, the problem of abnormal structure in wire bearing steel is solved, and the uniformity of network carbides and product quality are improved.
Patent Information
- Application Number
- CN202411014694.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing technology, it is difficult to control the hot-rolled structure and network carbides of wire rod bearing steel during the air-cooling process, which can easily lead to the generation of abnormal structures and affect product quality.
Adopting a four-stage air-cooling cooling mode, by reasonably controlling the spinning temperature, air-cooling roller speed and wire rod gap, it is divided into four stages: ultra-fast cooling, fast cooling, ultra-fast cooling and slow cooling, combined with air volume distribution to ensure carbonization The precipitation of substances is completed in the appropriate temperature range to avoid the generation of abnormal tissue.
It has improved the network carbide level of wire rod bearing steel, avoided the generation of abnormal structures such as martensite, and improved the finished product quality and subsequent processing stability.
Smart Images

Figure BDA0004965362410000101 
Figure BDA0004965362410000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of bearing steel metallurgy, and in particular relates to a control method that takes into account both the hot-rolled structure and the network carbide of wire bearing steel. Background Art
[0002] Bearing steel is a hypereutectoid steel, and it is inevitable that a large amount of carbides exist in the product. In the use of bearings, in addition to fatigue failure, there is also wear failure, so carbides cannot be absent. The key is how to improve the carbide uniformity index. The carbide uniformity index of bearing steel, especially the network carbide level, is an important factor affecting the fatigue life of its finished bearings. As we all know, wire bearing steel is quickly cooled after rolling so that it quickly passes through the temperature range where a large amount of carbides precipitate, which is beneficial to inhibit carbide precipitation and thus improve the network carbide index. However, due to the high C and Cr content of GCr15 bearing steel, rapid cooling after rolling can easily lead to the appearance of abnormal martensite structure in the hot-rolled structure of the wire rod. The existence of abnormal structure will cause certain troubles to both steel production companies and downstream processing companies.
[0003] In recent years, researchers have used different cooling methods to cool the wire rods after rolling of wire bearing steel to improve the carbide uniformity index of GCr15 bearing steel. The Chinese patent with the authorization announcement number CN109402356B discloses a controlled cooling and rolling method for controlling the network shape of carbides in bearing steel wire, including rapidly rolling the rods into wire rods of specified specifications and spinning them into loose coils, controlling the final rolling temperature at 780-880℃; controlling the spinning temperature at 750-850℃; using EDC water bath austempering cooling to control the continuous loose coils online, controlling the cooling rate at 2.0-10℃ / s, and controlling the final cooling temperature at 620-630℃; after EDC water bath austempering cooling, adding a hood for slow cooling, controlling the temperature out of the hood at 400-500℃; rolling up after slow cooling, and air cooling to room temperature. This patent combines the water bath isothermal quenching cooling and the insulation cover slow cooling of the wire rod after spinning, inhibiting the precipitation of carbides in the bearing steel during the cooling process, obtaining small strips or hemispherical carbides, and improving the network carbide index of the bearing steel. However, this method is not suitable for most steel production enterprises due to the uniqueness of the production equipment. The Chinese patent with the authorization announcement number CN110643798B discloses a method for controlling the network of carbides in the continuous casting GCr15 bearing steel wire rod. The control method optimizes the chemical composition of GCr15 by design; evaluates and grades the billet according to the superheat and low multiple before it is put into use, clarifies the feeding specifications according to the billet classification, and performs special control on the heating process. The downgraded billet appropriately prolongs the high temperature period of the furnace temperature ≥1150℃, and at the same time appropriately increases the rolling temperature, and strives to alleviate the segregation of the billet under the condition of long-term high-temperature diffusion; improves the coil air cooling process, and adjusts the coil in the air cooling process according to the size of the specification. The wire rod is quickly cooled from the spinning temperature to below 700℃ within 10 seconds, and then the wire rod is maintained at 630-700℃ for 10-15s and placed in the insulation cover, etc., to achieve effective control of the network carbides of the bearing steel. However, production practice shows that the cooling method in the patent cannot fully guarantee the network carbide index of the bearing steel, and improper operation will also cause abnormal organization in the hot-rolled wire rod. Therefore, how to obtain wire bearing steel that takes into account both hot-rolled structure and network carbide by air cooling under current technical conditions is a technical problem that needs to be urgently solved by technical personnel in this field. Summary of the invention
[0004] In order to solve the deficiencies in the prior art, the purpose of the present invention is to provide a control method for hot-rolled structure and network carbide of wire rod bearing steel. The production control method reasonably controls the spinning temperature, air cooling roller speed, wire rod gap, and reasonably distributes the air volume of the air cooling line fan on the high-speed wire rod production line to control the air cooling speed of the wire rod in different temperature ranges, and realizes a four-stage air cooling mode of "ultra-fast cooling + fast cooling + ultra-fast cooling + slow cooling", thereby obtaining a hot-rolled wire rod bearing steel with no abnormal structure and low network carbide level.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A control method for hot-rolled structure and network carbide of wire bearing steel, the control method comprising the following steps:
[0007] Step S1, placing the GCr15 bearing steel continuous casting billet into a heating furnace for heating and high-temperature diffusion to obtain product 1;
[0008] Step S2, subjecting the product 1 obtained in step S1 to rough rolling, intermediate rolling, pre-finishing rolling, finishing rolling, sizing, controlled rolling and controlled cooling, and then spinning, to roll the product 1 into a GCr15 wire rod with a diameter of 10-15 mm;
[0009] Step S3, cooling the wire rod obtained in step S2 in four stages on an air cooling line according to a temperature range;
[0010] Step S4: After air cooling, the wire rods are rolled and packaged, and the production is completed.
[0011] Preferably, the temperature of the high temperature diffusion in step S1 is 1200-1220° C., and the time of the high temperature diffusion is 90-110 min.
[0012] Preferably, in step S2, the temperature for starting the finish rolling is 960-980°C; the temperature for starting the sizing is 900-920°C; and the temperature for spinning is 860-870°C.
[0013] Preferably, the specific process of performing four-stage air cooling on the air cooling line of the wire rod in step S3 is as follows:
[0014] (1) The first stage of air cooling of the wire rod on the air cooling line is from spinning to the end position of the first fan, that is, the position 0-5m on the air cooling line
[0015] (2) The wire rod is cooled by air in the second stage on the air cooling line, and the length range on the air cooling line corresponds to the positions of the second and third fans, that is, the position of 5-15m on the air cooling line;
[0016] (3) The wire rod is cooled by air in the third stage on the air cooling line. The length range on the air cooling line corresponds to the position of the 4th and 5th fans, that is, the position of 15-25m on the air cooling line;
[0017] (4) The wire rod is cooled in the fourth stage of air cooling on the air cooling line. The wire rod is placed in a heat preservation cover for cooling, and the fan is completely turned off until the wire rod is under the air cooling line.
[0018] Preferably, the final cooling temperature of the wire rod in the first stage of air cooling is 780-790°C; the starting temperature of the wire rod in the second stage of air cooling is 780-790°C, and the final cooling temperature of the wire rod in the second stage of air cooling is 650-660°C; the starting temperature of the wire rod in the third stage of air cooling is 650-660°C, and the final cooling temperature of the wire rod in the third stage of air cooling is 580-600°C; the temperature of the wire rod out of the insulation cover in the fourth stage of air cooling is 450-480°C.
[0019] Preferably, the air-cooling roller speed of the first stage of air-cooling in step (1) is 0.5-0.52 m / s, the gap between two adjacent coils of wire rod is 30-32 mm, the wire rod running time is 9-11 s, and the wire rod cooling speed is controlled at 8-10°C / s.
[0020] Preferably, the air-cooling roller speed of the second stage of air-cooling in step (2) is 0.53-0.55 m / s, the gap between two adjacent coils of wire rod is 33-37 mm, the wire rod running time is 17-19 s, and the wire rod cooling speed is controlled at 6-8°C / s.
[0021] Preferably, the air-cooling roller speed of the third stage of air-cooling in step (3) is 0.58-0.60 m / s, the gap between two adjacent coils of wire rod is 37-43 mm, the wire rod running time is 15-17 s, and the wire rod cooling speed is controlled at 8-10°C / s.
[0022] The production control method of the present invention can take into account the mechanism of improving the generation of hot-rolled structure of wire bearing steel and the uniformity index of network carbide: for GCr15 bearing steel, Ar cmThe point temperature (referring to the temperature at which secondary cementite begins to precipitate from austenite during cooling) is about 900°C, the Ar1 point temperature (referring to the temperature at which austenite transforms to pearlite during cooling) is about 700°C, and the temperature range for large-scale precipitation of carbides is 700-850°C. Therefore, generally speaking, it is necessary to ensure rapid air cooling of the wire rod within this temperature range. The wire-spinning temperature of the present invention is selected to be 860-870°C in order to avoid large-scale precipitation of carbides before and during the wire-spinning process, and to ensure that the carbide precipitation process is completed on the air-cooling line. The first stage of air cooling is from spinning to the temperature of the wire rod dropping to 780℃. In the first stage, ultra-fast cooling is used to avoid carbide precipitation. The initial temperature of this stage is relatively high, and the cooling has not yet fully penetrated into the core of the wire rod, so the ultra-fast cooling method will not lead to excessive residual austenite structure, thereby avoiding the subsequent production of martensite structure; after entering the second stage of air cooling, the wire rod temperature is significantly reduced. If the ultra-fast cooling method is continued in this stage, the wire rod will be rapidly cooled to produce a central martensite structure. The reason for the production of martensite structure is that the temperature range of the second stage of air cooling is in the two-phase region of austenite + cementite. If it is cooled quickly at this time, the amount of carbide precipitation in the core of the wire rod will be reduced, resulting in more C and Cr elements still dissolved in the austenite structure, thereby improving the stability of the supercooled austenite structure and increasing the amount of residual austenite structure in the steel. After the wire rod is cooled to the Ms point temperature (referring to the temperature at which austenite begins to transform into martensite), martensite structure is generated in the core of the wire rod. At the same time, the precipitation of large amounts of carbides should also be avoided, so the cooling rate in this stage is appropriately reduced compared to the first stage, and a fast cooling method is adopted; after entering the third stage of air cooling, although ultra-fast cooling is adopted with a cooling rate close to that of the first stage of air cooling, the stability of the supercooled austenite structure has been determined by the second stage of air cooling, and the transformation of the austenite structure to the pearlite structure has begun in this stage. The production process in the present invention enables the stability of the supercooled austenite structure to meet the conditions for completing the transformation of the pearlite structure. The air cooling rate determines the size of the interlamellar spacing of the generated pearlite structure. Taking into account the different temperatures of the core and surface of the wire rod during the cooling process, the surface temperature of the wire rod after the final air cooling in this stage is set to 580°C, which can ensure that the wire rod as a whole quickly passes through the interval where a large amount of carbides precipitate; in the fourth stage of air cooling, the wire rod enters the insulation cover for slow cooling, which plays a role in eliminating stress and avoids failures such as breakage during subsequent wire rod transportation and processing.
[0023] Compared with the prior art, the present invention has the following positive and beneficial effects:
[0024] In the prior art, wire rod bearing steel is cooled in two stages on the air cooling line. In actual production, the air cooling intensity is often increased in order to pursue a low carbide network level, which can easily lead to the generation of abnormal structures such as martensite, affecting the use of subsequent products. The present invention adopts four-stage cooling, and adopts a relatively small cooling rate in the two-phase region of austenite + cementite, which can completely avoid the generation of abnormal structures such as martensite in the finished wire rod. At the same time, the overall air volume of the wire rod on the air cooling line is consistent with the overall air volume of the prior art, which means that the cooling rate of the wire rod is relatively faster in the secondary cementite precipitation stage, and less carbide precipitation, so the carbide network index of the finished wire rod will also be improved to a certain extent. DETAILED DESCRIPTION
[0025] The technical solution of the present invention is further described below in conjunction with the embodiments, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.
[0026] Example 1
[0027] A control method for hot-rolled structure and network carbide of wire bearing steel, the control method specifically comprises the following steps:
[0028] Step S1, placing a square GCr15 bearing steel continuous casting billet with a cross-sectional size of 150 mm into a heating furnace for heating, and diffusing it at a high temperature of 1210°C±10°C for 100min±10min to obtain product 1;
[0029] Step S2, the product 1 obtained above is subjected to rough rolling (the size of the rolled piece after rough rolling is about The rolling temperature is 1030-1060℃), intermediate rolling (the size of the rolled product after intermediate rolling is about The rolling temperature is 990-1020℃), pre-finishing rolling (the size of the rolled product after pre-finishing rolling is The rolling temperature is 970-1000℃), finishing rolling (the size of the rolled product after finishing rolling is The rolling temperature is 950-970℃), the diameter is reduced (the size of the rolled product after the diameter is reduced is The cross-sectional size of the product is continuously reduced, and the product 1 is rolled into a GCr15 wire with a diameter of 10 mm after controlled rolling and controlled cooling. At this time, the temperature of the product 1 entering the finishing mill is 960-980°C (i.e., the temperature of the product 1 starting to be finished is 960-980°C), the temperature of the product entering the sizing mill is 900-920°C (i.e., the temperature of the product 1 starting to be sizing is 900-920°C), and the temperature of the spinning is 860-870°C;
[0030] Step S3, the GCr15 wire obtained above is subjected to four-stage air cooling on the air cooling line according to the temperature range. At this time, the first five fans are turned on, and the speeds are 50%-30%-30%-50%-50% (the rated air volume of each fan is 230000m 3 / h, 50% speed means that 50% of the rated air volume can be provided, and 30% speed means that 30% of the rated air volume can be provided), the insulation cover opens the first 5; the specific process of the four-stage air cooling is as follows:
[0031] (1) The first stage of air cooling of GCr15 wire (wire rod) on the air cooling line starts from spinning to the end of the first fan, that is, the position of 0-5m on the air cooling line; the air cooling roller speed at this stage is 0.5-0.52m / s, the gap between two adjacent coils is 30-32mm, the coil travel time is 9-11s, the coil cooling speed is controlled at 8-10℃ / s, and the final cooling temperature of the coil is 780-790℃;
[0032] (2) The GCr15 wire (wire rod) is air-cooled in the second stage on the air-cooling line. The length range on the air-cooling line corresponds to the second and third fans, that is, the position of 5-15m on the air-cooling line; the air-cooling roller speed at this stage is 0.53-0.55m / s, the gap between two adjacent coils is 33-37mm, the coil travel time is 17-19s, the coil cooling speed is controlled at 6-8℃ / s, the starting temperature of the coil at this stage is 780-790℃, and the final cooling temperature of the coil is 650-660℃;
[0033] (3) The GCr15 wire (wire rod) is cooled by air in the third stage on the air cooling line. The length range on the air cooling line corresponds to the 4th and 5th fans, that is, the position of 15-25m on the air cooling line. Since the starting temperature of the wire rod at this stage (650-660℃) is lower than the Ar1 point temperature of the bearing steel (about 700℃), the transformation of austenite structure to pearlite structure begins to occur. Due to the release of latent heat of phase transformation, the wire rod will show an obvious "red return" phenomenon on the air cooling line, and the surface of the wire rod will return to about 720℃. The speed of the air cooling roller at this stage is 0.58-0.60m / s, the gap between two adjacent circles of wire rod is 37-43mm, the running time of the wire rod is about 15-17s, the cooling speed of the wire rod is controlled at 8-10℃ / s, the starting temperature of the wire rod at this stage is 650-660℃, and the final cooling temperature of the wire rod is 580-600℃.
[0034] (4) The GCr15 wire (wire rod) is cooled by air in the fourth stage on the air cooling line. The wire rod is placed in a heat preservation cover for natural and slow cooling. The initial cooling temperature of the wire rod entering the heat preservation cover at this stage is 580-600°C, and the temperature of the wire rod out of the heat preservation cover is 450-480°C;
[0035] Step S4: After the four stages of air cooling are completed, the wire rods are rolled and packaged, and the production is completed to obtain wire bearing steel.
[0036] Example 2
[0037] A control method for hot-rolled structure and network carbide of wire bearing steel, the control method specifically comprises the following steps:
[0038] Step S1, placing a square GCr15 bearing steel continuous casting billet with a cross-sectional size of 150 mm into a heating furnace for heating, and diffusing it at a high temperature of 1210° C.±10° C. for 100 min±10 min to obtain product 1;
[0039] Step S2, the product 1 obtained above is subjected to rough rolling (the size of the rolled piece after rough rolling is about The rolling temperature is 1030-1060℃), intermediate rolling (the size of the rolled product after intermediate rolling is about The rolling temperature is 990-1020℃), pre-finishing rolling (the size of the rolled product after pre-finishing rolling is The rolling temperature is 970-1000℃), the diameter is reduced (the size of the rolled product after the diameter is reduced is The cross-sectional size of the product is continuously reduced, and the product 1 is rolled into a GCr15 wire with a diameter of 15 mm after controlled rolling and controlled cooling. At this time, the temperature of the product 1 entering the sizing unit is 900-920°C (that is, the temperature of the product 1 entering the sizing unit is 900-920°C), and the temperature of the spinning is 860-870°C;
[0040] Step S3, the GCr15 wire obtained above is subjected to four-stage air cooling on the air cooling line according to the temperature range. At this time, the first six fans are turned on, and the speeds are 70%-50%-50%-70%-70%-70% (the rated air volume of each fan is 230000m 3 / h, a speed of 70% means that it can provide 70% of the rated air volume, and a speed of 50% means that it can provide 50% of the rated air volume), and the insulation cover opens the first 6; the specific process of the four-stage air cooling is as follows:
[0041] (1) The first stage of air cooling of GCr15 wire (wire rod) on the air cooling line is from spinning to the end position of the first fan, that is, the position of 0-5m on the air cooling line; the air cooling roller speed at this stage is 0.5-0.52m / s, the gap between two adjacent coils is 30-32mm, the coil travel time is 9-11s, the coil cooling speed is controlled at 8-10℃ / s, and the final cooling temperature of the coil is 780-790℃;
[0042] (2) The GCr15 wire (wire rod) is air-cooled in the second stage on the air-cooling line. The length range on the air-cooling line corresponds to the position of the second and third fans, that is, the position of 5-15m on the air-cooling line; the air-cooling roller speed at this stage is 0.53-0.55m / s, the gap between two adjacent coils is 33-37mm, the coil travel time is 17-19s, the coil cooling speed is controlled at 6-8℃ / s, the starting temperature of the coil at this stage is 780-790℃, and the final cooling temperature of the coil is 650-660℃;
[0043] (3) GCr15 wire (wire rod) is cooled by air in the third stage on the air cooling line. The length range on the air cooling line corresponds to the position of the 4th and 5th fans, that is, the position of 15-25m on the air cooling line. Since the starting temperature of the wire rod at this stage (650-660℃) is lower than the Ar1 point temperature of the bearing steel (about 700℃), the transformation of austenite structure to pearlite structure begins to occur. Due to the release of latent heat of phase transformation, the wire rod will show an obvious "red return" phenomenon on the air cooling line, and the surface of the wire rod will return to about 720℃. At this stage, the speed of the air cooling roller is 0.58-0.60m / s, the gap between two adjacent circles of wire rod is 37-43mm, the running time of the wire rod is about 15-17s, the cooling speed of the wire rod is controlled at 8-10℃ / s, the starting temperature of the wire rod at this stage is 650-660℃, and the final cooling temperature of the wire rod is 580-600℃.
[0044] (4) The GCr15 wire (wire rod) is cooled by air in the fourth stage on the air cooling line, and the wire rod is placed in a heat preservation cover for slow cooling. The initial cooling temperature of the wire rod entering the heat preservation cover at this stage is 580-600°C, and the temperature of the wire rod out of the heat preservation cover is 450-480°C;
[0045] Step S4: After the four stages of air cooling are completed, the wire rods are rolled and packaged, and the production is completed to obtain wire bearing steel.
[0046] Comparative Example 1
[0047] A control method for taking into account the hot-rolled structure and network carbide of wire bearing steel, which is exactly the same as the control method in Example 1, except that in step S3, the number of fans and insulation covers turned on and the speed of the fans are different when the GCr15 wire is subjected to four-stage air cooling on the air cooling line according to the temperature range. In this comparative example, in step S3, the first 4 fans are turned on, the speed is 50%, and the first 4 insulation covers are turned on.
[0048] Comparative Example 2
[0049] A control method that takes into account the hot-rolled structure and network carbide of wire bearing steel is exactly the same as the control method in Example 2, except that in step S3, the number of fans and insulation covers turned on and the speed of the fans are different when the GCr15 wire is subjected to four-stage air cooling on the air cooling line according to the temperature range. In this comparative example, in step S3, the first 5 fans are turned on, the speed is 70%, and the first 5 insulation covers are turned on.
[0050] Comparative Example 3
[0051] A control method for taking into account both the hot-rolled structure and the network carbide of wire bearing steel, which is exactly the same as the control method in Example 2, except that the spinning temperature of the GCr15 wire in step S2 is different. In this comparative example, the spinning temperature in step S2 is 800-810°C.
[0052] Comparative Example 4
[0053] A control method that takes into account the hot-rolled structure and network carbide of wire bearing steel, which is exactly the same as the control method in Example 2, except that the air-cooling roller speed when the GCr15 wire is air-cooled in stages on the air-cooling line according to the temperature range in step S3 and the gap between two adjacent circles of wire rods are different (the gap between wire rods is determined by the roller speed), in this comparative example, in step S3, the first-stage roller speed on the air-cooling line is 0.35-0.37 m / s, and the wire rod gap is 15-17 mm; the second-stage roller speed is 0.37-0.39 m / s, and the wire rod gap is 18-22 mm; the third-stage roller speed is 0.42-0.45 m / s, and the wire rod gap is 22-28 mm.
[0054] Test example
[0055] The wire bearing steels obtained in Examples 1-2 and Comparative Examples 1-4 of the present invention were subjected to metallographic examination. Five samples were taken from each Example and Comparative Example to conduct hot rolling structure and network carbide examinations. The specific examination results are shown in Tables 1 and 2, respectively.
[0056] Table 1 Hot rolling microstructure test results of wire bearing steel in Examples 1-2 and Comparative Examples 1-4
[0057]
[0058] Table 2 Test results of network carbides of wire bearing steel in Examples 1-2 and Comparative Examples 1-4
[0059]
[0060] It can be seen from the results in Table 1 that the hot-rolled structures of the wire produced in Example 1 and Example 2 are both P+Fe3C, while the abnormal structure M appears in the core structure of the finished hot-rolled materials produced in Comparative Examples 1 and 2. It can be seen from the results in Table 2 that the level of the wire network carbide produced in the embodiment is better than that in the comparative example. In summary, the production control method of the present invention that takes into account the hot-rolled structure and network carbide of the wire bearing steel is implemented. By reasonably controlling the spinning temperature, the air-cooling roller speed, the wire rod gap, and the reasonable allocation of the air volume of the air-cooling line fan, a four-stage air-cooling mode of "ultra-fast cooling + fast cooling + ultra-fast cooling + slow cooling" is achieved. Under the premise of ensuring the network carbide index, the abnormal structure in the finished wire bearing steel is avoided, thereby improving the quality of the wire bearing steel product and the stability of subsequent deep processing.
[0061] Obviously, the above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from them are still within the protection scope of the invention.
Claims
1. A control method for hot-rolled structure and network carbide of wire bearing steel, It is characterized in that The control method comprises the following steps: Step S1, placing the GCr15 bearing steel continuous casting billet into a heating furnace for heating and high-temperature diffusion to obtain product 1; Step S2, subjecting the product 1 obtained in step S1 to rough rolling, intermediate rolling, pre-finishing rolling, finishing rolling, sizing, controlled rolling and controlled cooling, and then spinning, to roll the product 1 into a GCr15 wire rod with a diameter of 10-15 mm; Step S3, cooling the wire rod obtained in step S2 in four stages on an air cooling line according to a temperature range; Step S4: After air cooling, the wire rods are rolled and packaged, and the production is completed.
2. According to claim 1, a control method for hot-rolled structure and network carbide of wire rod bearing steel is taken into consideration. It is characterized in that The temperature of the high temperature diffusion in step S1 is 1200-1220° C., and the time of the high temperature diffusion is 90-110 min.
3. According to claim 1, a control method for hot-rolled structure and network carbide of wire rod bearing steel is taken into consideration. It is characterized in that In step S2, the temperature for starting the finish rolling is 960-980°C; the temperature for starting the sizing is 900-920°C; and the temperature for spinning is 860-870°C.
4. According to claim 1, a control method for hot-rolled structure and network carbide of wire rod bearing steel is taken into consideration. It is characterized in that The specific process of the wire rod being subjected to four-stage air cooling on the air cooling line in step S3 is as follows: (1) The first stage of air cooling of the wire rod on the air cooling line starts from spinning to the end of the first fan, which is the position 0-5m on the air cooling line; (2) The wire rod is cooled by air in the second stage on the air cooling line, and the length range on the air cooling line corresponds to the second and third fans, that is, the position of 5-15m on the air cooling line; (3) The wire rod is cooled by air in the third stage on the air cooling line. The length range on the air cooling line corresponds to the position of the 4th and 5th fans, that is, the position of 15-25m on the air cooling line; (4) The wire rod is cooled by air in the fourth stage on the air cooling line. The wire rod is placed in a heat preservation cover for natural cooling with the fan turned off until the wire rod is under the air cooling line.
5. A control method for hot-rolled structure and network carbide of wire rod bearing steel according to claim 4, It is characterized in that The final cooling temperature of the wire rod in the first stage of air cooling is 780-790°C; the starting temperature of the wire rod in the second stage of air cooling is 780-790°C, and the final cooling temperature of the wire rod in the second stage of air cooling is 650-660°C; the starting temperature of the wire rod in the third stage of air cooling is 650-660°C, and the final cooling temperature of the wire rod in the third stage of air cooling is 580-600°C; the temperature of the wire rod out of the insulation cover in the fourth stage of cooling is 450-480°C.
6. A control method for hot-rolled structure and network carbide of wire rod bearing steel according to claim 4, It is characterized in that In the step (1), the speed of the air-cooled roller in the first stage of air-cooling is 0.5-0.52 m / s, the gap between two adjacent coils of wire rod is 30-32 mm, the wire rod running time is 9-11 s, and the wire rod cooling speed is controlled at 8-10°C / s.
7. A control method for hot-rolled structure and network carbide of wire rod bearing steel according to claim 4, It is characterized in that In the step (2), the speed of the air-cooled roller in the second stage of air-cooling is 0.53-0.55 m / s, the gap between two adjacent coils is 33-37 mm, the coil running time is 17-19 s, and the coil cooling speed is controlled at 6-8 °C / s.
8. A control method for hot-rolled structure and network carbide of wire rod bearing steel according to claim 4, It is characterized in that In the step (3), the speed of the air-cooled roller in the third stage of air-cooling is 0.58-0.60 m / s, the gap between two adjacent coils is 37-43 mm, the coil running time is 15-17 s, and the coil cooling speed is controlled at 8-10°C / s.
Citation Information
Patent Citations
Continuous casting GCr15 bearing steel wire rod carbide mesh control method
CN110643798A
Production method of bearing steel coil
CN111926163A
Production method for tire cord steel
CN113909295A
Method for controlling network carbide of GCr15 bearing steel wire rod
CN113981193A
Step cooling method of high carbon wire rod for inhibiting generation of martensite
KR1019990055107A
Cited By
Controlled cooling process for improving network carbide of wire rod
CN119614827A
Method for suppressing network carbide of bearing steel high speed wire rod during rolling
CN123079736A