Composite solid electrolyte and preparation method and application thereof
By using porous structural pore-forming materials and polyacrylonitrile to form an integrated surface layer in solid-state batteries, the problem of high contact resistance between solid electrolytes and solid electrodes is solved, battery performance and conductivity are improved, and the battery is suitable for industrial production.
Patent Information
- Application Number
- CN202410884133.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-01
AI Technical Summary
In solid-state lithium batteries, the contact resistance between the solid-state electrolyte and the solid-state electrode is large, which affects the battery performance. The existing methods have strict process requirements and are difficult to meet the needs of industrial production.
By arranging a pore-forming material with a porous structure on the surface of the inorganic solid electrolyte and forming an integrated surface layer with polyacrylonitrile, the interface resistance between the inorganic solid electrolyte and polyacrylonitrile is reduced, a continuous conductive path is formed, and the ionic conductivity is improved.
It effectively reduces the contact resistance between the solid electrolyte and the solid electrode, improves the ionic conductivity and cycle life of the composite solid electrolyte, simplifies the preparation process, and has industrial prospects.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of solid electrolytes, and in particular to a composite solid electrolyte and a preparation method and application thereof. Background Art
[0002] Solid-state lithium batteries are gaining more and more attention due to their high safety. Compared with the liquid electrolytes used in traditional lithium-ion batteries, solid electrolytes have the advantages of low flammability, high thermal stability, no leakage, and low explosion risk. As the core component of solid-state lithium batteries, they can fundamentally eliminate the safety hazards of battery smoke, fire and explosion caused by leakage, thereby greatly improving the safety of lithium batteries.
[0003] The structure of a solid-state lithium battery includes a positive electrode, a solid electrolyte and a negative electrode. Different from the solid / liquid contact of a traditional liquid lithium-ion battery, the solid electrolyte and the solid electrode are in solid / solid contact and lack wettability. Therefore, the solid / solid interface has a higher contact impedance, which seriously affects the performance of the battery.
[0004] In order to reduce the contact impedance between the solid electrolyte and the solid electrode in the solid-state lithium battery and improve the performance of the solid-state lithium battery, a lot of efforts have been made in this field. For example: Chinese invention patent CN108695558 discloses an all-solid-state battery core and a high-performance all-solid-state battery containing the battery core. The positive electrode material, negative electrode material, electrolyte and current collector of the solid-state battery are integrated into one body, thereby eliminating the interface between the four and avoiding the generation of interface impedance. However, the method disclosed in patent CN108695558 has strict requirements on the process, otherwise there will still be an interface between the positive electrode material, negative electrode material, electrolyte and current collector, and there will still be a large interface impedance. At the same time, the room temperature ionic conductivity of the all-solid-state battery prepared by the invention is low, which is difficult to meet the current needs.
[0005] As a solid electrolyte, polymer solid electrolytes (SPEs) have good electrochemical stability against metallic lithium, a wide electrochemical window and high mechanical strength. However, existing polymer solid electrolytes still have certain technical defects, such as high crystallinity, low ionic conductivity at room temperature, and narrow electrochemical window. At present, various methods are used to reduce the crystallinity of polymer solid electrolytes to improve ionic conductivity, such as synthesizing new polymer solid electrolytes with low glass transition temperature, structural cross-linking, and introducing organic plasticizers or inorganic fillers. However, these methods are relatively complicated to implement and cannot meet the production needs of industry. Summary of the invention
[0006] In order to reduce the contact impedance between the solid electrolyte and the solid electrode in a solid-state lithium battery and improve the performance of the solid-state lithium battery, the present invention provides a composite solid electrolyte and its preparation method and application. The present invention arranges a pore-forming material with a porous structure on the surface of an inorganic solid electrolyte, and forms an integrated surface layer with polyacrylonitrile on the surface of the inorganic solid electrolyte, thereby reducing the surface impedance of the inorganic solid electrolyte. As a polymer solid electrolyte, polyacrylonitrile has a large crystallinity that increases its interface impedance. The addition of the pore-forming material causes more micropores to exist in the polypropylene layer when it forms an integrated surface layer with polyacrylonitrile, thereby reducing the interface impedance of the polypropylene layer. At the same time, due to the arrangement of the pore-forming material in the surface layer, a continuous conductive path can be formed in the surface layer, thereby increasing the ionic conductivity of the composite solid electrolyte.
[0007] The specific technical scheme of the present invention is: In a first aspect, the present invention provides a method for preparing a composite solid electrolyte, comprising the following steps: Step S1: providing a pore-forming material, wherein the pore-forming material has a porous structure; Step S2: placing the pore-forming material on the surface of the inorganic solid electrolyte; Step S3: a polyacrylonitrile layer is provided on the surface of the inorganic solid electrolyte, and the pore-forming material and the polyacrylonitrile layer form an integrated surface layer to obtain a composite solid electrolyte.
[0008] In a solid-state battery, there is a large contact impedance between the solid electrolyte and the solid electrode. The present invention arranges a pore-forming material with a porous structure on the surface of an inorganic solid electrolyte, and forms an integrated surface layer with polyacrylonitrile on the surface of the inorganic solid electrolyte, thereby reducing the surface impedance of the inorganic solid electrolyte. As a polymer solid electrolyte, polyacrylonitrile has a large crystallinity that increases its interface impedance. The addition of the pore-forming material causes more micropores to exist in the polypropylene layer when it forms an integrated surface layer with polyacrylonitrile, thereby reducing the interface impedance of the polypropylene layer. At the same time, due to the arrangement of the pore-forming material in the surface layer, a continuous conductive path can be formed in the surface layer, thereby increasing the ionic conductivity of the composite solid electrolyte.
[0009] As a preferred embodiment of the above preparation method, the pore-forming material is selected from one or more of covalent organic framework materials COFs, metal-organic framework materials MOFs, nickel fibers, and aluminum foams.
[0010] The functions of the pore-forming material are as follows: first, it is arranged on the surface of the inorganic solid electrolyte as a contact bridge between the inorganic electrolyte and the solid electrode, reducing the contact impedance between the inorganic solid electrolyte and the solid electrode; second, it forms an integrated surface layer with polyacrylonitrile to reduce the contact impedance of polyacrylonitrile, so that the ions have a lower impedance when conducting between the solid electrolyte and the solid electrode. Therefore, in addition to the requirement of having a porous structure, the pore-forming material needs to have the characteristics of excellent conductive properties in order to further improve the electrical properties of the composite solid electrolyte. The pore-forming material is selected from one or more of covalent organic framework materials COFs, metal-organic framework materials MOFs, nickel fibers, and aluminum foams, which can make the composite solid electrolyte have a higher ionic conductivity.
[0011] As a preferred embodiment of the above preparation method, the inorganic solid electrolyte is selected from one or more of lithium lanthanum titanium oxide, lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide and lithium aluminum titanium phosphate.
[0012] As a preferred embodiment of the above preparation method, the mass ratio of the pore-forming material to the inorganic solid electrolyte is 0.5 to 4:100.
[0013] The pore-forming material plays a vital role in the composite solid electrolyte provided by the present invention, and its mass content in the composite solid electrolyte affects the final performance of the composite solid electrolyte. In the composite solid electrolyte, the mass ratio of the pore-forming material to the inorganic solid electrolyte is preferably 0.5 to 4:100.
[0014] As a preferred embodiment of the above preparation method, the mass ratio of the polyacrylonitrile to the inorganic solid electrolyte is 12 to 25:100.
[0015] The polyacrylonitrile layer is arranged on the surface of the inorganic solid electrolyte, which can greatly reduce the contact impedance between the inorganic solid electrolyte and the solid electrode. The pore-forming material and the polyacrylonitrile form an integrated surface layer, which can form a conductive path between the inorganic solid electrolyte and the solid electrode in the polyacrylonitrile, further improving the ionic conductivity of the composite solid electrolyte, and at the same time, reducing the contact impedance of the polyacrylonitrile layer itself. Therefore, the mass content of the polyacrylonitrile layer in the composite solid electrolyte will affect the final performance of the composite solid electrolyte. In the present composite solid electrolyte, it is appropriate to make the mass ratio of polyacrylonitrile to the inorganic solid electrolyte be 12 to 25:100.
[0016] Specifically, step S2 is: uniformly mixing the pore-forming material and the inorganic solid electrolyte, and hot pressing them to disperse and adhere the pore-forming material to the surface of the inorganic solid electrolyte.
[0017] Specifically, step S3 is: infiltrating the mixture of the hot-pressed pore-forming material and the inorganic solid electrolyte with a polyacrylonitrile dispersion, drying, and hot-pressing again to obtain a composite solid electrolyte.
[0018] Preferably, the pressure of the second hot pressing is 0.5 to 1.8 MPa, and the time of the second hot pressing is 2 to 10 minutes.
[0019] In a second aspect, the present invention provides a composite solid electrolyte prepared by the above preparation method.
[0020] In a third aspect, the present invention provides the use of the composite solid electrolyte prepared by the above preparation method in the preparation of an all-solid-state battery.
[0021] Compared with the prior art, the present invention has the following technical effects: (1) The present invention arranges a pore-forming material with a porous structure on the surface of an inorganic solid electrolyte, and forms an integrated surface layer with polyacrylonitrile on the surface of the inorganic solid electrolyte, thereby reducing the surface impedance of the inorganic solid electrolyte. As a polymer solid electrolyte, polyacrylonitrile has a large crystallinity that increases its interface impedance. The addition of the pore-forming material causes more micropores to exist in the polypropylene layer when the pore-forming material forms an integrated surface layer with polyacrylonitrile, thereby reducing the interface impedance of the polypropylene layer. At the same time, due to the arrangement of the pore-forming material in the surface layer, a continuous conductive path can be formed in the surface layer, thereby increasing the ionic conductivity of the composite solid electrolyte.
[0022] (2) Based on the structural setting of the composite solid electrolyte, the present invention further optimizes the selection of pore-forming materials, the amount of pore-forming materials, and the amount of polyacrylonitrile, so that the ion conductivity of the composite solid electrolyte is further improved. And for the composite solid electrolyte of the present invention, the preparation process of the composite solid electrolyte is optimized, so that the composite solid electrolyte has a longer cycle life.
[0023] (3) The preparation process provided by the present invention is simple and has industrial prospects. DETAILED DESCRIPTION
[0024] The present invention will be further described below in conjunction with embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should belong to the scope of protection of the present invention.
[0025] The present invention provides a method for preparing a composite solid electrolyte, comprising the following steps: Step S1: providing a pore-forming material, wherein the pore-forming material has a porous structure; Step S2: placing the pore-forming material on the surface of the inorganic solid electrolyte; Step S3: a polyacrylonitrile layer is provided on the surface of the inorganic solid electrolyte, and the pore-forming material and the polyacrylonitrile layer form an integrated surface layer to obtain a composite solid electrolyte.
[0026] In a solid-state battery, there is a large contact impedance between the solid electrolyte and the solid electrode. The present invention arranges a pore-forming material with a porous structure on the surface of an inorganic solid electrolyte, and forms an integrated surface layer with polyacrylonitrile on the surface of the inorganic solid electrolyte, thereby reducing the surface impedance of the inorganic solid electrolyte. As a polymer solid electrolyte, polyacrylonitrile has a large crystallinity that increases its interface impedance. The addition of the pore-forming material causes more micropores to exist in the polypropylene layer when it forms an integrated surface layer with polyacrylonitrile, thereby reducing the interface impedance of the polypropylene layer. At the same time, due to the arrangement of the pore-forming material in the surface layer, a continuous conductive path can be formed in the surface layer, thereby increasing the ionic conductivity of the composite solid electrolyte.
[0027] As a preferred embodiment of the above preparation method, the pore-forming material is selected from one or more of covalent organic framework materials COFs, metal-organic framework materials MOFs, nickel fibers, and aluminum foams.
[0028] The functions of the pore-forming material are as follows: first, it is arranged on the surface of the inorganic solid electrolyte as a contact bridge between the inorganic electrolyte and the solid electrode, reducing the contact impedance between the inorganic solid electrolyte and the solid electrode; second, it forms an integrated surface layer with polyacrylonitrile to reduce the contact impedance of polyacrylonitrile, so that the ions have a lower impedance when conducting between the solid electrolyte and the solid electrode. Therefore, in addition to the requirement of having a porous structure, the pore-forming material needs to have the characteristics of excellent conductive properties in order to further improve the electrical properties of the composite solid electrolyte. The pore-forming material is selected from one or more of covalent organic framework materials COFs, metal-organic framework materials MOFs, nickel fibers, and aluminum foams, which can make the composite solid electrolyte have a higher ionic conductivity.
[0029] As a preferred embodiment of the above preparation method, the inorganic solid electrolyte is selected from one or more of lithium lanthanum titanium oxide, lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide and lithium aluminum titanium phosphate.
[0030] As a preferred embodiment of the above preparation method, the mass ratio of the pore-forming material to the inorganic solid electrolyte is 0.5 to 4:100.
[0031] As a preferred embodiment of the above preparation method, the mass ratio of the polyacrylonitrile to the inorganic solid electrolyte is 12 to 25:100.
[0032] Example 1 This embodiment provides a composite solid electrolyte, which is prepared according to the following steps: (1) 100 parts of LLZTO solid electrolyte powder and 2 parts of aluminum foam powder were mixed and ground evenly, and then hot-pressed at 50° C. and a pressure of 10 MPa for 3 min to disperse and adhere the pore-forming material aluminum foam to the surface of the LLZTO solid electrolyte to obtain a pre-composite inorganic solid electrolyte.
[0033] (2) Disperse 18 parts of polyacrylonitrile in an appropriate amount of N,N-dimethylacetamide to obtain a polyacrylonitrile dispersion.
[0034] (3) The pre-composite inorganic solid electrolyte is soaked with polyacrylonitrile dispersion, and then placed in an oven for drying at 80°C. After being taken out, it is hot-pressed again at 60°C. The hot-pressing pressure is 0.8 MPa and the time is 6 minutes. The pore-forming material aluminum foam and polyacrylonitrile form an integrated surface layer on the surface of the LLZTO solid electrolyte, thereby obtaining a composite solid electrolyte.
[0035] Example 2 This embodiment provides a composite solid electrolyte, which is prepared according to the following steps: (1) 100 parts of LLZTO solid electrolyte powder and 0.5 parts of aluminum foam powder were mixed and ground evenly, and then hot-pressed at 50° C. and a pressure of 10 MPa for 3 min to disperse and adhere the pore-forming material aluminum foam to the surface of the LLZTO solid electrolyte to obtain a pre-composite inorganic solid electrolyte.
[0036] (2) Disperse 12 parts of polyacrylonitrile in an appropriate amount of N,N-dimethylacetamide to obtain a polyacrylonitrile dispersion.
[0037] (3) The pre-composite inorganic solid electrolyte is soaked with polyacrylonitrile dispersion, and then placed in an oven for drying at 80°C. After being taken out, it is hot-pressed again at 60°C. The hot-pressing pressure is 0.5 MPa and the time is 10 min. The pore-forming material aluminum foam and polyacrylonitrile form an integrated surface layer on the surface of the LLZTO solid electrolyte, thereby obtaining a composite solid electrolyte.
[0038] Example 3 This embodiment provides a composite solid electrolyte, which is prepared according to the following steps: (1) 100 parts of LLZTO solid electrolyte powder and 4 parts of aluminum foam powder were mixed and ground evenly, and then hot-pressed at 50° C. and a pressure of 10 MPa for 3 min to disperse and adhere the pore-forming material aluminum foam to the surface of the LLZTO solid electrolyte to obtain a pre-composite inorganic solid electrolyte.
[0039] (2) Disperse 25 parts of polyacrylonitrile in an appropriate amount of N,N-dimethylacetamide to obtain a polyacrylonitrile dispersion.
[0040] (3) The pre-composite inorganic solid electrolyte is infiltrated with a polyacrylonitrile dispersion, and then placed in an oven for drying at 80°C. After being taken out, it is hot-pressed again at 60°C. The hot-pressing pressure is 1.8 MPa and the time is 2 min. The pore-forming material aluminum foam and polyacrylonitrile form an integrated surface layer on the surface of the LLZTO solid electrolyte, thereby obtaining a composite solid electrolyte.
[0041] Example 4 This embodiment provides a composite solid electrolyte, which is prepared according to the following steps: (1) 100 parts of LLZTO solid electrolyte powder and 2 parts of nickel fiber powder were mixed and ground evenly, and then hot-pressed at 50° C. and 10 MPa for 3 min to disperse and adhere the pore-forming material nickel fiber to the surface of the LLZTO solid electrolyte to obtain a pre-composite inorganic solid electrolyte.
[0042] (2) Disperse 18 parts of polyacrylonitrile in an appropriate amount of N,N-dimethylacetamide to obtain a polyacrylonitrile dispersion.
[0043] (3) The pre-composite inorganic solid electrolyte is soaked with polyacrylonitrile dispersion, and then placed in an oven for drying at 80°C. After being taken out, it is hot-pressed again at 60°C. The hot-pressing pressure is 0.8 MPa and the time is 6 min. The pore-forming material nickel fiber and polyacrylonitrile form an integrated surface layer on the surface of the LLZTO solid electrolyte, thereby obtaining a composite solid electrolyte.
[0044] Example 5 This embodiment provides a composite solid electrolyte, which is prepared according to the following steps: (1) 100 parts of LLZTO solid electrolyte powder and 2 parts of covalent organic framework material COFs powder were mixed and ground evenly, and then hot-pressed at 50°C and a pressure of 10 MPa for 3 min to disperse and adhere the pore-forming material covalent organic framework material COFs to the surface of the LLZTO solid electrolyte to obtain a pre-composite inorganic solid electrolyte.
[0045] (2) Disperse 18 parts of polyacrylonitrile in an appropriate amount of N,N-dimethylacetamide to obtain a polyacrylonitrile dispersion.
[0046] (3) The pre-composite inorganic solid electrolyte is soaked in the polyacrylonitrile dispersion, and then placed in an oven for drying at 80°C. After being taken out, it is hot-pressed again at 60°C. The hot-pressing pressure is 0.8 MPa and the time is 6 minutes. The pore-forming material covalent organic framework material COFs and polyacrylonitrile form an integrated surface layer on the surface of the LLZTO solid electrolyte, thereby obtaining a composite solid electrolyte.
[0047] Example 6 This embodiment provides a composite solid electrolyte, which is prepared according to the following steps: (1) 100 parts of LLZTO solid electrolyte powder and 2 parts of metal-organic framework material MOFs powder were mixed and ground evenly, and then hot-pressed at 50°C and a pressure of 10 MPa for 3 min to disperse and adhere the pore-forming material metal-organic framework material MOFs to the surface of the LLZTO solid electrolyte to obtain a pre-composite inorganic solid electrolyte.
[0048] (2) Disperse 18 parts of polyacrylonitrile in an appropriate amount of N,N-dimethylacetamide to obtain a polyacrylonitrile dispersion.
[0049] (3) The pre-composite inorganic solid electrolyte is soaked in the polyacrylonitrile dispersion, and then placed in an oven for drying at 80°C. After being taken out, it is hot-pressed again at 60°C. The hot-pressing pressure is 0.8 MPa and the time is 6 minutes. The pore-forming material metal-organic framework material MOFs and polyacrylonitrile form an integrated surface layer on the surface of the LLZTO solid electrolyte, thereby obtaining a composite solid electrolyte.
[0050] Comparative Example 1 The main difference between this comparative example and Example 1 is that in step (1), 0.1 parts of aluminum foam is added. The other steps are the same as those in Example 1.
[0051] Comparative Example 2 The main difference between this comparative example and Example 1 is that in step (1), 6 parts of aluminum foam are added. The other steps are the same as those in Example 1.
[0052] Comparative Example 3 The main difference between this comparative example and Example 1 is that in step (2), 8 parts of polyacrylonitrile are added. The other steps are the same as those in Example 1.
[0053] Comparative Example 4 The main difference between this comparative example and Example 1 is that in step (2), 30 parts of polyacrylonitrile are added. The other steps are the same as those in Example 1.
[0054] Comparative Example 5 The main difference between this comparative example and Example 1 is that in step (3), the pressure of the second hot pressing is 0.2 MPa. The other steps are the same as those in Example 1.
[0055] Comparative Example 6 The main difference between this comparative example and Example 1 is that in step (3), the pressure of the second hot pressing is 3 MPa. The other steps are the same as those in Example 1.
[0056] Performance test The composite solid electrolyte prepared in Examples 1 to 6 and Comparative Examples 1 to 6 was used as the electrolyte to assemble button-type solid-state lithium batteries, and the room temperature ionic conductivity and cycle performance were tested. The results are shown in Table 1. The test conditions for room temperature ionic conductivity are: at room temperature of 25°C, 0.1C charging, 0.1C discharging, and a charge and discharge range of 3.0 to 4.3V. The test conditions for cycle performance are: at room temperature of 25°C, 0.3C charging, 0.3C discharging, and a charge and discharge range of 3.0 to 4.3V. The cycle test was performed to determine the number of cycles required for the capacity to reach 80% of the initial capacity.
[0057] Table 1 <![CDATA[Ionic conductivity (*10 -4 S / cm)]]> Cycle life (weeks) Example 1 7.34 657 Example 2 7.32 650 Example 3 7.39 653 Example 4 8.20 741 Example 5 7.81 706 Example 6 7.97 740 Comparative Example 1 1.48 391 Comparative Example 2 3.02 512 Comparative Example 3 1.64 311 Comparative Example 4 1.59 378 Comparative Example 5 1.96 114 Comparative Example 6 2.07 362 From the test data in Table 1, we can see that: (1) The present invention arranges a pore-forming material with a porous structure on the surface of an inorganic solid electrolyte, and forms an integrated surface layer with polyacrylonitrile on the surface of the inorganic solid electrolyte, thereby reducing the surface impedance of the inorganic solid electrolyte. The resulting composite solid electrolyte has high conductivity.
[0058] The principle of high ionic conductivity of the composite solid electrolyte provided by the present invention is analyzed as follows: polyacrylonitrile, as a polymer solid electrolyte, has a large crystallinity which increases its interfacial impedance. The addition of pore-forming material causes more micropores to exist in the polypropylene layer when it forms an integrated surface layer with polyacrylonitrile, thereby reducing the interfacial impedance of the polypropylene layer. At the same time, due to the arrangement of the pore-forming material in the surface layer, a continuous conductive path can be formed in the surface layer, thereby increasing the ionic conductivity of the composite solid electrolyte.
[0059] (2) By comparing comparative examples 1 to 2 with Example 1, it can be seen that the pore-forming materials added in comparative examples 1 to 2 are 0.1 parts and 6 parts respectively. When the composite solid electrolyte prepared in comparative examples 1 to 2 is used to assemble a solid-state battery, its ionic conductivity is reduced to varying degrees, especially when the amount of pore-forming material added is small, the ionic conductivity is significantly reduced. The reason for this is that when a continuous conductive path is formed in the surface layer, a sufficient amount of pore-forming material is required. When the amount of pore-forming material set on the surface of the inorganic solid electrolyte is small, the conductive effect will be significantly reduced. It can be seen that in this composite solid electrolyte, it is appropriate to make the mass ratio of pore-forming material to inorganic solid electrolyte be 0.5 to 4:100.
[0060] (3) Comparative Examples 3 to 4 and Example 1 show that the polyacrylonitrile added in Comparative Examples 3 to 4 is 8 parts and 30 parts respectively. When the composite solid electrolyte prepared in Comparative Examples 3 to 4 is used to assemble a solid-state battery, its ionic conductivity is greatly reduced, and the cycle performance is reduced. The reason is that the polyacrylonitrile layer is arranged on the surface of the inorganic solid electrolyte, which can greatly reduce the contact impedance between the inorganic solid electrolyte and the solid electrode. The pore-forming material and the polyacrylonitrile form an integrated surface layer, which can form a conductive path between the inorganic solid electrolyte and the solid electrode in the polyacrylonitrile, further improving the ionic conductivity of the composite solid electrolyte. At the same time, the contact impedance of the polyacrylonitrile layer itself is reduced. Therefore, the mass content of the polyacrylonitrile layer in the composite solid electrolyte will affect the final performance of the composite solid electrolyte. It can be seen that in this composite solid electrolyte, it is appropriate to make the mass ratio of polyacrylonitrile to the inorganic solid electrolyte be 12 to 25:100.
[0061] (3) From the comparative analysis of Comparative Examples 5 to 6 and Example 1, it can be seen that the hot pressing pressures of Comparative Examples 5 to 6 when forming the integrated surface layer are 0.2Mpa and 3MPa respectively. When the composite solid electrolyte prepared in Comparative Examples 5 to 6 is used to assemble a solid-state battery, its cycle performance is significantly reduced, especially when the hot pressing pressure is 0.2Mpa, the cycle performance is significantly reduced, and the ionic conductivity of Comparative Examples 5 to 6 is greatly reduced. It can be seen that the hot pressing pressure when forming the integrated surface layer may have a greater impact on the integrated surface layer formed by polyacrylonitrile and the pore-forming material. When the pore-forming material forms a continuous conductive path in the surface layer, it needs to be formed under an appropriate hot pressing pressure. Excessive or too small hot pressing pressure will affect the interaction between the surface layer and the inorganic solid electrolyte. And further from the comparative analysis of Comparative Examples 5 to 6 and Example 1, it can be seen that the pressure of the second hot pressing is preferably 0.5 to 1.8MPa.
[0062] (4) From the comparative analysis of Example 1 and Examples 4 to 6, it can be seen that different pore-forming materials may also have an impact on the electrical properties of the composite solid electrolyte.
[0063] The metal-organic framework material MOFs used in the present invention is ZIF-8, which was purchased from Xi'an Ruixi Biotechnology Co., Ltd.; the covalent organic framework material COFs used in the present invention was purchased from Xi'an Ruixi Biotechnology Co., Ltd.
[0064] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0065] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a composite solid electrolyte, characterized in that: The following steps are involved: Step S1: providing a pore-forming material, wherein the pore-forming material has a porous structure; Step S2: placing the pore-forming material on the surface of the inorganic solid electrolyte; Step S3: a polyacrylonitrile layer is provided on the surface of the inorganic solid electrolyte, and the pore-forming material and the polyacrylonitrile layer form an integrated surface layer to obtain a composite solid electrolyte.
2. The method for preparing a composite solid electrolyte according to claim 1, characterized in that: The pore-forming material is selected from one or more of nickel fiber, aluminum foam, covalent organic framework material COFs, and metal-organic framework material MOFs.
3. The method for preparing a composite solid electrolyte according to claim 1, characterized in that: The inorganic solid electrolyte is selected from one or more of lithium lanthanum titanium oxide, lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide and lithium aluminum titanium phosphate.
4. The method for preparing a composite solid electrolyte according to claim 1, characterized in that: The mass ratio of the pore-forming material to the inorganic solid electrolyte is 0.5 to 4:
100.
5. The method for preparing a composite solid electrolyte according to claim 1, characterized in that: The mass ratio of the polyacrylonitrile to the inorganic solid electrolyte is 12 to 25:
100.
6. The method for preparing a composite solid electrolyte according to claim 1, characterized in that: Step S2 is: uniformly mixing the pore-forming material and the inorganic solid electrolyte, and hot pressing them to disperse and adhere the pore-forming material to the surface of the inorganic solid electrolyte.
7. The method for preparing a composite solid electrolyte according to claim 6, characterized in that: Step S3 is: infiltrating the mixture of the hot-pressed pore-forming material and the inorganic solid electrolyte with a polyacrylonitrile dispersion, drying, and hot-pressing again to obtain a composite solid electrolyte.
8. The method for preparing a composite solid electrolyte according to claim 7, characterized in that: The pressure of the second hot pressing is 0.5 to 1.8 MPa, and the time of the second hot pressing is 2 to 10 minutes.
9. The composite solid electrolyte prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the composite solid electrolyte prepared by the preparation method according to any one of claims 1 to 8, or the composite solid electrolyte according to claim 9 in the preparation of an all-solid-state battery.
Citation Information
Patent Citations
Multi-layer composite solid electrolyte, preparation method thereof and all-solid-state lithium battery
CN113363559A
Composite solid electrolyte of MOFs-based polymer protective layer as well as preparation method and application of composite solid electrolyte
CN117410557A