Conductive polymer composition and use thereof
Through the combination of polythiophene and organic solvent-dispersible metals, a polymer composition with low surface resistance is designed to solve the problem of high surface resistance of existing conductive polymer films, achieve high electromagnetic wave shielding and hygrothermal durability, and provide excellent transparency and conductivity.
Patent Information
- Application Number
- CN202380024511.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-01-18
- Filing Date
- 2023-03-10
- Publication Date
- 2024-10-15
AI Technical Summary
Existing conductive polymer films have high surface resistance during film production, which limits their application scope.
A polymer composition composed of polythiophene and organic solvent-dispersed metals (such as silver nanowires) is used to reduce the surface resistance through specific structural unit and dopant design, and form a conductive polymer film through drying treatment.
Significantly reduces the surface resistance of the conductive polymer film, improves its electromagnetic wave shielding properties and moist heat durability, while providing excellent transparency and conductivity.
Smart Images

Figure CN118786178A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a conductive polymer composition and its application. Background Art
[0002] Conductive polymer materials in which electron-withdrawing compounds are doped as dopants in π-conjugated polymers represented by polyacetylene, polythiophene, polyaniline or polypyrrole are being developed. The above-mentioned conductive polymer materials are being studied for use in, for example, antistatic agents, solid electrolytes for capacitors, conductive coatings, electromagnetic wave shielding materials, electrochromic devices, electrode materials, thermoelectric conversion materials, transparent conductive films, chemical sensors, actuators, etc. In such applications, some materials require high compatibility with resins, and some materials are afraid of water, so conductive polymer compositions whose solvents are organic solvents are required.
[0003] As conductive polymers that are dissolved in an organic solvent, for example, polyaniline-type conductive polymers and polythiophene-type conductive polymers are known (for example, Patent Document 1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2019-210356 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] The organic solvent-based conductive polymer composition disclosed in Patent Document 1 has a problem that the conductive polymer film tends to have a relatively high surface resistance during film formation, and thus has limited uses.
[0009] An object of the present invention is to provide an organic solvent-based conductive polymer composition capable of producing a conductive polymer film having a lower surface resistance than conventionally known compositions.
[0010] Solutions to the problem
[0011] The present inventors have conducted intensive studies to solve the above-mentioned problems and, as a result, have found the conductive polymer composition shown below, thereby completing the present invention.
[0012] That is, the present invention relates to the following conductive polymer composition and conductive polymer film. The conductive polymer film produced using the above composition can be used as, for example, a transparent electrode and a transparent conductive film.
[0013] [1] A conductive polymer composition comprising:
[0014] Polythiophene (A) 0.01 to 10% by weight,
[0015] 0.01 to 1.0 wt% of an organic solvent dispersible metal (B), and
[0016] Organic solvent (C),
[0017] The polythiophene (A) comprises at least one structural unit selected from the structural unit represented by the following general formula (1) and the structural unit represented by the following general formula (2),
[0018]
[0019] [In the above general formulas (1) and (2), R 2 is a hydrogen atom, a methyl group, an ethyl group, a linear or branched alkyl group having 3 to 6 carbon atoms, or a fluorine atom; m is an integer of 1 to 10; n is 0 or 1; M + represents an organic ammonium ion or a quaternary ammonium ion. ].
[0020] [2] The conductive polymer composition according to [1], wherein
[0021] The organic solvent dispersible metal (B) is at least one organic solvent dispersible metal selected from the group consisting of silver nanoparticles, silver nanoplates, silver nanowires, copper nanoparticles, copper nanoplates, and copper nanowires.
[0022] [3] The conductive polymer composition according to [1] or [2], wherein
[0023] The organic solvent dispersible metal (B) is organic solvent dispersible silver nanowires.
[0024] [4] The conductive polymer composition according to any one of [1] to [3], wherein
[0025] The content of the polythiophene (A) is 0.1 to 5% by mass.
[0026] [5] The conductive polymer composition according to any one of [1] to [4], wherein
[0027] The content of the organic solvent-dispersible metal (B) is 0.01 to 100 parts by mass relative to 1 part by mass of the polythiophene (A).
[0028] [6] A film forming method, the method comprising:
[0029] The conductive polymer composition described in any one of [1] to [5] is applied onto a support and then dried.
[0030] [7] A film comprising:
[0031] Polythiophene (A),
[0032] Organic solvent dispersible metal (B),
[0033] The polythiophene (A) comprises at least one structural unit selected from the structural unit represented by the following general formula (1) and the structural unit represented by the following general formula (2),
[0034]
[0035] [In the above general formulas (1) and (2), R 2 is a hydrogen atom, a methyl group, an ethyl group, a linear or branched alkyl group having 3 to 6 carbon atoms, or a fluorine atom; m is an integer of 1 to 10; n is 0 or 1; M + represents an organic ammonium ion or a quaternary ammonium ion. ].
[0036] Effects of the Invention
[0037] The present invention can provide an organic solvent-based conductive polymer composition capable of producing a conductive polymer film having a lower surface resistance than conventionally known compositions. DETAILED DESCRIPTION
[0038] An embodiment of the present invention is described in detail below. It should be noted that, in this specification, "~" represents a numerical range including both end values as the lower limit and the upper limit.
[0039] As described above, the conductive polymer composition of the present invention can provide a conductive polymer film with lower surface resistance than the conventionally known composition. In addition, the conductive polymer film has excellent uniformity of film quality and exhibits excellent electromagnetic wave shielding properties. Therefore, compared to the conventional technology, the conductive polymer composition of the present invention has achieved remarkable effects.
[0040] In addition, as will be described in detail below, the conductive polymer composition of the present invention exhibits excellent wet heat durability and can significantly suppress the wet heat degradation of organic solvent-dispersible metals, achieving a remarkable effect in this regard.
[0041] Furthermore, the conductive polymer composition of the present invention exhibits high conductivity and can provide a conductive polymer film having excellent transparency, thereby being able to provide an electromagnetic wave shielding film with minimal coloration and discoloration, achieving a remarkable effect in this respect.
[0042] In addition, the conductive polymer composition of the present invention can provide a highly transparent resistor film on the surface of an electromagnetic wave absorber, and achieves a remarkable effect in this regard.
[0043] One embodiment of the present invention relates to a conductive polymer composition comprising:
[0044] Polythiophene (A) 0.01 to 10% by weight,
[0045] 0.01 to 1.0 wt% of an organic solvent dispersible metal (B), and
[0046] Organic solvent (C),
[0047] The polythiophene (A) comprises at least one structural unit selected from the structural unit represented by the following general formula (1) and the structural unit represented by the following general formula (2),
[0048]
[0049] [In the above general formulas (1) and (2), R 2 is a hydrogen atom, a methyl group, an ethyl group, a linear or branched alkyl group having 3 to 6 carbon atoms, or a fluorine atom; m is an integer of 1 to 10; n is 0 or 1; M + represents an organic ammonium ion or a quaternary ammonium ion.]
[0050] In the above general formulas (1) and (2), R 2 It is a hydrogen atom, a methyl group, an ethyl group, a linear or branched alkyl group having 3 to 6 carbon atoms, or a fluorine atom.
[0051] The straight-chain or branched alkyl group having 3 to 6 carbon atoms is not particularly limited, and examples thereof include n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, neopentyl, tert-pentyl, cyclopentyl, n-hexyl, 2-ethylbutyl and cyclohexyl.
[0052] From the perspective of film forming properties, the above R 2 It is preferably a hydrogen atom, a methyl group, an ethyl group or a fluorine atom, and more preferably a hydrogen atom or a methyl group.
[0053] In the above general formulae (1) and (2), m represents an integer of 1 to 10, and is preferably an integer of 1 to 6, more preferably an integer of 1 to 4, and even more preferably 2 or 3 from the viewpoint of film-forming properties.
[0054] In the above general formulae (1) and (2), n represents 0 or 1, and is preferably 1 from the viewpoint of excellent conductivity.
[0055] The structural unit represented by the general formula (2) represents the doping state of the structural unit represented by the general formula (1). The doping state is exhibited by the sulfonic acid group or sulfonate group in the structural unit represented by the general formula (1) acting as a p-type dopant.
[0056] Dopants that cause insulator-metal transfer due to doping can be divided into electron acceptors and electron donors. The former enters near the polymer chain of the conductive polymer by doping, taking away π electrons from the conjugated system of the main chain, and as a result, positive charges (holes) are injected into the main chain, so they are also called p-type dopants. In addition, the latter in turn provides electrons to the conjugated system of the main chain, and these electrons move in the conjugated system of the main chain, so they are also called n-type dopants.
[0057] The dopant in the present invention is a sulfonic acid group or a sulfonate group covalently bonded to the polymer molecule, and is a p-type dopant. A polymer that can generate conductivity without adding a dopant from the outside is called a self-doping polymer.
[0058] In the above general formulas (1) and (2), M + It represents an organic ammonium ion or a quaternary ammonium ion.
[0059] The organic ammonium ion is not particularly limited, and examples thereof include [NH(R 3 )(R 4 )2] + It should be noted that the above R 3 represents an alkyl group having 1 to 20 carbon atoms or an alkyl group having a total of 1 to 20 carbon atoms and having a substituent. 4 Each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an alkyl group having 1 to 20 carbon atoms in total and having a substituent.
[0060] The alkyl group having 1 to 20 carbon atoms is not particularly limited, and examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, neopentyl, tert-pentyl, cyclopentyl, n-hexyl, isohexyl, 2-ethylbutyl, cyclohexyl, n-heptyl, isohexyl, methylhexyl, n-octyl, isooctyl, methylheptyl, ethylhexyl, n-nonyl, n-decyl, ethyloctyl, butylhexyl, n-undecyl, n-dodecyl, n-hexadecyl, n-heptadecyl, octylnonyl, n-octadecyl, n-nonadecyl, n-eicosyl, and octyldodecyl.
[0061] Examples of the alkyl group having 1 to 20 carbon atoms in total and having a substituent include alkyl groups having 7 to 20 carbon atoms containing a halogen atom, an amino group or a hydroxyl group, and specific examples include trifluoromethyl, 2-hydroxyethyl, 8-hydroxyoctyl or 9-aminononyl.
[0062] Among them, as a substituent R 3From the perspective of easily exerting high conductivity, it is preferred that each independently represents an alkyl group having 1 to 12 carbon atoms, more preferably each independently represents an alkyl group having 6 to 12 carbon atoms, still more preferably each independently represents an alkyl group having 6 to 8 carbon atoms, and further preferably each independently represents an n-hexyl group, an isohexyl group, an n-octyl group or an isooctyl group.
[0063] In addition, as a substituent R 4 From the perspective of easily exerting high conductivity, it is preferred that each independently represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, more preferably each independently represents a hydrogen atom or an alkyl group having 6 to 12 carbon atoms, still more preferably each independently represents a hydrogen atom or an alkyl group having 6 to 8 carbon atoms, and further preferably each independently represents a hydrogen atom, n-hexyl, isohexyl, n-octyl or isooctyl.
[0064] The organic ammonium ion is not particularly limited, and examples thereof include n-heptylamine, di-n-heptylamine, tri-n-heptylamine, n-octylamine, di-n-octylamine, di-iso-octylamine, tri-n-octylamine, tri-iso-octylamine, di-n-hexylamine, tri-n-hexylamine, n-nonylamine, di-n-nonylamine, tri-n-nonylamine, n-decylamine, di-n-decylamine, tri-n-decylamine, n-dodecylamine, di-n-dodecylamine, tri-n-dodecylamine, n-hexadecylamine, di-n-hexadecylamine, tri-n-hexadecylamine, n-octadecylamine, di-n-octadecylamine, tri-n-octadecylamine, n-eicosylamine, di-n-eicosylamine, tri-n-eicosylamine, di-n-hexylamine, tri-n-hexadecylamine, Hexylamine, N-methyl-N,N-di-n-octylamine, N-methyl-N,N-di-isooctylamine, or N-methyl-N,N-di-n-hexylamine, N,N-dimethyl-n-heptylamine, N,N-dimethyl-n-octylamine, N,N-dimethyl-n-nonylamine, N,N-dimethyl-n-decylamine, N,N-dimethyl-n-dodecylamine, N,N-dimethyl-n-hexadecylamine, N,N-dimethyl-n-octadecylamine, N,N-dimethyl-n-icosylamine, N,N-diethyl-n-heptylamine, N,N-diethyl-n-octylamine, N,N-diethyl-n-nonylamine, N, N-diethyl-n-decylamine, N,N-diethyl-n-dodecylamine, N,N-diethyl-n-hexadecylamine, N,N-diethyl-n-octadecylamine, N,N-diethyl-n-icosylamine, N-methyl-N-hexylamine, N-methyl-N-heptylamine, N-methyl-N-octylamine, N-methyl-N-nonylamine, N-methyl-N-dodecylamine, N-methyl-N-hexadecylamine, N-methyl-N-octadecylamine, N-ethyl-N-hexylamine, N-ethyl-N-heptylamine, N-ethyl-N-octylamine, N-ethyl -N-n-nonylamine, N-ethyl-N-dodecylamine, N-ethyl-N-hexadecylamine, N-ethyl-N-octadecylamine, 7-hydroxyheptylamine, 8-hydroxyoctylamine, 9-hydroxynonylamine, 10-hydroxydecylamine, 12-hydroxydodecylamine, 16-hydroxyhexadecylamine, 18-hydroxyoctadecylamine, 20-hydroxyicosylamine, 7-aminoheptylamine, 8-aminooctylamine, 9-aminononylamine, 10-aminodecylamine, 12-aminododecylamine, 16-aminohexadecylamine, 18-aminooctadecylamine or 20-aminoicosylamine, etc.
[0065] Among the above-mentioned organic ammonium ions, from the perspective of excellent film-forming properties, preferred are di-n-octylamine, di-iso-octylamine, tri-n-octylamine, tri-iso-octylamine, di-n-hexylamine, tri-n-hexylamine, N-methyl-N,N-di-n-octylamine, N-methyl-N,N-di-iso-octylamine, N-methyl-N,N-di-n-hexylamine, N-isopropyl-N,N-dimethylamine, or N-n-butyl-N,N-dimethylamine.
[0066] The quaternary ammonium ion is not particularly limited, and examples thereof include tetramethylammonium, tetraethylammonium, tetra-n-propylammonium, tetra-n-butylammonium, and tetra-n-hexylammonium.
[0067] The structural unit represented by the above formula (1) or (2) is not particularly limited, and specific examples thereof include 6-(2,3-dihydro-thieno[3,4-b][1,4]dihydro- alkyl-2-yl)hexane-1-sulfonic acid, 8-(2,3-dihydro-thieno[3,4-b][1,4]di 2-Alkane) octane-1-sulfonic acid, 3-(dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-propanesulfonic acid, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-methyl-1-propanesulfonic acid, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy)]-1-ethyl-1-propanesulfonic acid, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-propyl-1-propanesulfonic acid, 4-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-methyl-1-butanesulfonic acid, 6-(2,3-dihydro-thieno[3,4-b][1,4]di 6-(2,3-dihydro-thieno[3,4-b][1,4]diol)hexane-1-sulfonic acid dioctylamine salt, 6-(2,3-dihydro-thieno[3,4-b][1,4]diol)hexane-1-sulfonic acid diisooctylamine salt, 6-(2,3-dihydro-thieno[3,4-b][1,4]diol)-1-sulfonic acid tri-n-octylamine salt alkyl-2-yl)hexane-1-sulfonic acid triisooctylamine salt, 8-(2,3-dihydro-thieno[3,4-b][1,4]di alkyl-2-yl) octane-1-sulfonic acid dioctylamine salt, 8-(2,3-dihydro-thieno[3,4-b][1,4]di 2-Alkane-2-yl) octane-1-sulfonic acid diisooctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-propanesulfonic acid dioctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-propanesulfonic acid diisooctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-methyl-1-propanesulfonic acid dioctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-ethyl-1-propanesulfonic acid dioctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-propyl-1-propanesulfonic acid dioctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-butyl-1-propanesulfonic acid dioctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-pentyl-1-propanesulfonic acid dioctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-hexyl-1-propanesulfonic acid dioctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-isopropyl-1-propanesulfonic acid dioctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-isobutyl-1-propanesulfonic acid dioctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-isopentyl-1-propanesulfonic acid dioctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-fluoro-1-propanesulfonic acid dioctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-methyl-1-propanesulfonic acid dioctylamine salt, 3-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-methyl-1-propanesulfonic acid dioctylamine salt, 4-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-butanesulfonic acid dioctylamine salt, 4-[(2,3-dihydrothieno[3,4-b][1,4]di alkyl-2-yl)methoxy]-1-methyl-1-butanesulfonic acid dioctylamine salt or 4-[(2,3-dihydrothieno[3,4-b][1,4]di [(2-((((((((((((((((((-((-1-(-1,(-1,(-2-( ...
[0068] Regarding the polythiophene (A) of the present invention containing at least one structural unit selected from the structural unit represented by the above general formula (1) and the structural unit represented by the above general formula (2), it is preferred that the polythiophene (A) contains two or more of at least one structural unit selected from the structural unit represented by the above general formula (1) and the structural unit represented by the above general formula (2) repeatedly, and it is more preferred that the polythiophene (A) is composed of at least one structural unit selected from the structural unit represented by the above general formula (1) and the structural unit represented by the above general formula (2) and is composed of two or more of the structural units repeated.
[0069] In the present invention, the electrical conductivity of the polythiophene (A) is not particularly limited, but is preferably 0.01 S / cm or more as the electrical conductivity (electrical conductivity) in a thin film state.
[0070] In addition, as the polythiophene (A) in the present invention, those synthesized based on known information can be used.
[0071] In the conductive polymer composition of the present invention, the concentration of the polythiophene (A) containing at least one structural unit selected from the structural unit represented by the above general formula (1) and the structural unit represented by the above general formula (2) is in the range of 0.01 to 10 wt %, based on the total amount of the conductive polymer composition as 100 wt %. It should be noted that from the viewpoint of excellent conductivity and workability, the concentration of the polythiophene (A) in the conductive polymer composition of the present invention is preferably in the range of 0.02 to 7 wt %, more preferably in the range of 0.03 to 5 wt %, still more preferably in the range of 0.03 to 3 wt %, and further preferably in the range of 0.03 to 2 wt %.
[0072] The conductive polymer composition of the present invention contains an organic solvent dispersible metal (B), and the concentration of the organic solvent dispersible metal (B) is 0.01 to 1.0 wt % based on the total amount of the conductive polymer composition being 100 wt %. Based on this feature, a coating film with high electrical conductivity can be obtained.
[0073] The organic solvent dispersible metal (B) is not particularly limited, and specific examples thereof include organic solvent dispersible silver particles or organic solvent dispersible copper particles. The shapes of these organic solvent dispersible metals are not particularly limited, and shapes such as particles, fillers, plates, rods, triangular pyramids, cubes, tubes, wires, fibers, or microparticles can be used.
[0074] In addition, the above-mentioned organic solvent-dispersible metal (B) is preferably at least one organic solvent-dispersible metal selected from the group consisting of silver nanoparticles, silver nanoplates, silver nanowires, copper nanoparticles, copper nanoplates and copper nanowires from the viewpoint of excellent conductivity, and is more preferably organic solvent-dispersible silver nanowires from the viewpoint of storage stability.
[0075] The preferred size of the organic solvent dispersible metal (B) varies based on its shape. For example, for nanoparticles, a particle diameter of 1 to 1000 nm is preferred. For nanowires, a length of 1 to 50 μm is preferred. For nanofibers, a diameter of 1 to 100 nm and a length of more than 100 times the diameter are preferred. For nanorods, a diameter of 1 to 100 nm and a length of 20 to 100 times the diameter are preferred. For nanocubes, each piece is preferably 1 to 200 nm long. For nanoplates, a thickness of 1 to 100 nm and a width of 2 to 20 times the thickness are preferred.
[0076] It should be noted that the organic solvent-dispersible metal (B) refers to a metal dispersed or dispersible in an organic solvent. That is, the conductive polymer composition of the present invention can be produced by mixing a paste of the organic solvent-dispersible metal (B), or by mixing an organic solvent dispersion of the organic solvent-dispersible metal (B). When the conductive polymer composition is produced by mixing an organic solvent dispersion of the organic solvent-dispersible metal (B), the organic solvent contained in the organic solvent dispersion may be a component of the organic solvent (C).
[0077] The conductive polymer composition of the present invention contains 0.01 to 1.0 wt% of an organic solvent-dispersible metal (B), and this content refers to the content of the organic solvent-dispersible metal (B) itself. That is, when the conductive polymer composition of the present invention is produced using an organic solvent dispersion of the organic solvent-dispersible metal (B), components such as the solvent contained in the organic solvent dispersion are not included in the content of the organic solvent-dispersible metal (B).
[0078] The content of the organic solvent-dispersible metal (B) is preferably 0.05 to 0.9 wt %, more preferably 0.08 to 0.8 wt %, from the viewpoint of high compatibility with the conductive polymer and ability to maintain high conductivity.
[0079] The content of the organic solvent-dispersible metal (B) relative to 1 part by mass of the polythiophene (A) is not particularly limited, but is preferably 0.01 to 100 parts by mass, more preferably 0.05 to 20 parts by mass, and even more preferably 0.1 to 10 parts by mass.
[0080] The organic solvent (C) is not particularly limited, and examples thereof include alcohol solvents (e.g., methanol, ethanol, n-propanol, isopropanol, n-butanol, 1-butanol, isobutanol, tert-butanol, ethylene glycol, etc.); aromatic hydrocarbon solvents (benzene, toluene, xylene, etc.); ketone solvents (acetone, methyl ethyl ketone, methyl propyl ketone, methyl isobutyl ketone, diacetone alcohol, etc.); ether solvents (ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, 1,4-dioxane, etc.); glycol ester solvents (ethylene glycol monoethyl ether acetate, propylene glycol, etc.); Monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, etc.); glycol ether solvents (diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, etc.); halogenated solvents (chloroform, dichloromethane, 1,2-dichloroethane, chlorobenzene, etc.); amide solvents (N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, dimethylimidazolidinone, hexamethylphosphoric acid triamide, etc.) or sulfur-containing solvents (dimethyl sulfoxide, cyclopentane, etc.).
[0081] These organic solvents (C) may be used alone or in combination of two or more.
[0082] In addition, the above-mentioned organic solvent (C) is preferably one or more organic solvents selected from ethanol, isopropanol, 1-butanol, methyl isobutyl ketone, methyl ethyl ketone, N-methyl-2-pyrrolidone and propylene glycol monomethyl ether from the perspective of excellent compatibility with the resin.
[0083] Note that, as described above, the organic solvent (C) may contain an organic solvent contained in the organic solvent dispersion of the organic solvent-dispersible metal (B).
[0084] The concentration (content) of the organic solvent (C) in the conductive polymer composition of the present invention is not particularly limited, but is preferably within a range of 80 to 99.9 wt %, more preferably 85 to 99.8 wt %, from the viewpoint of excellent processability.
[0085] Likewise, the content of the organic solvent (C) is not particularly limited, but is preferably 10 to 3000 parts by mass, more preferably 50 to 2000 parts by mass, and even more preferably 100 to 1500 parts by mass, relative to 1 part by mass of the polythiophene (A).
[0086] The conductive polymer composition of the present invention may further contain other additives (D) in addition to the above-mentioned polythiophene (A), the organic solvent-dispersible metal (B) and the organic solvent (C).
[0087] The other additive (D) is not particularly limited, and examples thereof include a binder and a surfactant, etc. It should be noted that the other additive (D) may be used alone or in combination of two or more.
[0088] The binder is not particularly limited, and examples thereof include vinyl pyrrolidone resin, acrylic resin, polyurethane resin, methyl methacrylate resin, styrene-butadiene resin, vinyl acetate resin, polyamide resin, phenolic resin, epoxy resin, melamine resin, thermosetting polyimide, cellulose nitrate or other cellulose resins, or polyvinyl alcohol resin, etc. Examples of the curing method include thermal curing and UV curing.
[0089] The above-mentioned binder is preferably at least one selected from vinyl pyrrolidone resin, polyurethane resin, acrylic resin and epoxy resin from the viewpoint of excellent film-forming property.
[0090] The content of the binder relative to 1 part by mass of the polythiophene (A) is not particularly limited, but is preferably 1 to 1500 parts by mass, more preferably 1 to 1000 parts by mass, and still more preferably 1 to 500 parts by mass.
[0091] The surfactant is not particularly limited, and examples thereof include polymeric nonionic surfactants, amphoteric surfactants, fluorine-based surfactants, silicone-based surfactants, and acetylene glycol-based surfactants.
[0092] The above-mentioned amphoteric surfactant is not particularly limited, and for example, betaine-type amphoteric surfactants can be cited. The betaine-type amphoteric surfactant is not particularly limited, and for example, alkyl dimethyl betaine, dodecyl dimethyl betaine, octadecyl dimethyl betaine, dodecyl dihydroxyethyl betaine, etc. can be cited.
[0093] As the fluorine-based surfactant, a surfactant having a perfluoroalkyl group is preferred, but is not particularly limited, and examples thereof include perfluoroalkanes, perfluoroalkyl carboxylic acids, perfluoroalkyl sulfonic acids, and perfluoroalkyl ethylene oxide adducts.
[0094] The above-mentioned silicone-based surfactant is not particularly limited, and examples thereof include polyether-modified polydimethylsiloxane, polyether ester-modified polydimethylsiloxane, hydroxyl-containing polyether-modified polydimethylsiloxane, acrylic group-containing polyether-modified polydimethylsiloxane, acrylic group-containing polyester-modified polydimethylsiloxane, perfluoropolyether-modified polydimethylsiloxane, perfluoropolyester-modified polydimethylsiloxane or silicone-modified acrylic compound.
[0095] Fluorine-based surfactants and organic silicon surfactants as leveling agents are effective in improving the flatness of the coating film.
[0096] It should be noted that the content of the surfactant is not particularly limited, but is preferably 0.0001 to 1 part by mass, more preferably 0.001 to 1 part by mass, and still more preferably 0.001 to 0.1 part by mass, relative to 1 part by mass of the polythiophene (A).
[0097] The conductive polymer composition of the present embodiment is not particularly limited and can be produced by mixing the components by a common method. For example, it is preferably produced according to the following procedure.
[0098] Step 1: An aqueous solution of a polymer composed of a structural unit represented by the following general formula (2) and a structural unit represented by the following general formula (3) is produced by a conventionally known production method.
[0099]
[0100] [In the above general formulas (2) and (3), R 2 , m and n are the same as R in the above general formulas (1) and (2) 2 , m and n have the same meaning.]
[0101] Step 2: Add an organic amine compound or its solution as the source of the organic ammonium ions, or an alcohol solution of a quaternary ammonium compound as the source of the quaternary ammonium ions, to the aqueous solution of the polymer, and obtain a polythiophene (A) containing at least one structural unit selected from the structural unit represented by the general formula (1) and the structural unit represented by the general formula (2) by mixing and stirring.
[0102] Step 3: The solvent is removed from the mixture in step 2 to obtain the above-mentioned polythiophene (A) as a solid.
[0103] Step 4: The solid polythiophene (A) obtained in step 3, the organic solvent-dispersible metal (B) and the organic solvent (C) are mixed in any order by a generally known method, and further, additives (D) other than those mentioned above are mixed and stirred as needed to obtain the conductive polymer composition of this embodiment.
[0104] The step 1 is not particularly limited, and can be carried out, for example, by subjecting a known monomer compound to oxidative polymerization by a conventionally known method and then subjecting the compound to an acid treatment according to a conventionally known method.
[0105] It should be noted that, for the above-mentioned steps 2 to 3, from the perspective of obtaining a conductive polymer composition with excellent conductivity, after the above-mentioned polythiophene (A) reacts with an organic amine compound or a quaternary ammonium ion in water and / or an alcohol solvent, it is preferably combined with solvent washing, reprecipitation, centrifugal sedimentation, ultrafiltration, dialysis, ion exchange resin treatment and the like as needed.
[0106] As the organic amine compound, an organic amine compound obtained by removing the conjugate acid of the organic ammonium ion can be used.
[0107] The quaternary ammonium compound is not particularly limited, and examples thereof include tetramethylammonium chloride, tetraethylammonium chloride, tetra-n-propylammonium chloride, tetra-n-butylammonium chloride, and tetra-n-hexylammonium chloride.
[0108] The alcohol solvent is not particularly limited, and examples thereof include methanol, ethanol, propanol, isopropanol, butanol, isobutanol, tert-butanol, pentanol, isopentanol, hexanol, isohexanol, cyclohexanol, octanol, 2-ethylhexanol, ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, hexylene glycol, ethylene glycol monomethyl ether or ethylene glycol monoethyl ether.
[0109] The above step 4 is characterized in that the solid of the above polythiophene (A), the organic solvent dispersible metal (B) and the organic solvent (C) are mixed, but at this time, the above other additives (D) may be further added and mixed as needed. It should be noted that, from the perspective of operability, it is more preferable to dissolve the above materials (A), (B) and (D) in the organic solvent (C) before mixing. There is no particular limitation on the order of adding and mixing the above materials, and the conductive polymer composition of the present invention can be prepared by mixing these materials in any order.
[0110] Here, the temperature during mixing is not particularly limited, and for example, the mixing can be carried out at room temperature to under heating, preferably at 0°C or higher and 40°C or lower.
[0111] The atmosphere during mixing is not particularly limited, and the mixture may be mixed in the air or in an inert gas, and is preferably mixed in an inert gas.
[0112] In addition, as a mixing method, a general mixing and dissolving operation performed by a stirring blade, a stirring blade, etc. can be cited. In addition to such a mixing and dissolving operation, ultrasonic irradiation or homogenization treatment (for example, using a mechanical homogenizer, an ultrasonic homogenizer, a high-pressure homogenizer, etc.) can also be performed. During the homogenization treatment, in order to prevent thermal degradation of the polymer, it is preferably treated at a low temperature.
[0113] The viscosity (viscosity at 20° C.) of the conductive polymer composition of the present invention is preferably 200 mPA·s or less, more preferably 100 mPA·s or less, and further preferably 50 mPA·s or less.
[0114] In the conductive polymer composition of the present invention, the concentration of each component can be adjusted by adjusting the mixing ratio or by concentrating or diluting after mixing. The concentration method may be a method of distilling off the solvent under reduced pressure or a method using an ultrafiltration membrane.
[0115] In the conductive polymer composition of the present invention, the concentration of all components except the solvent is preferably in the range of 0.5 to 20% by weight, more preferably in the range of 0.5 to 15% by weight.
[0116] The method for forming a conductive polymer film from the conductive polymer composition of the present invention is not particularly limited, and examples thereof include a method in which the conductive polymer composition of the present invention is applied onto a support and then dried.
[0117] The above-mentioned support is not particularly limited as long as it is a support to which the conductive polymer composition of the present embodiment can be coated, and for example, a polymer support or an inorganic support can be cited. The polymer support is not particularly limited, and for example, thermoplastic resins, nonwoven fabrics, paper, etc. can be cited. As thermoplastic resins, for example, polyethylene, polypropylene, polyethylene terephthalate, polyacrylate, polycarbonate, and polyimide can be cited. As nonwoven fabrics, for example, natural fibers or synthetic fibers can be cited. As paper, paper whose main component is general cellulose can be cited. As inorganic supports, there are no particular limitations, and for example, glass, glass fiber, ceramics, aluminum oxide, or tantalum oxide can be cited.
[0118] Examples of the method for coating the conductive polymer composition include casting, dipping, wire bar coating, dispenser coating, roll coating, gravure coating, flexographic printing, screen printing, and offset printing.
[0119] The drying temperature of the coating is not particularly limited as long as it is a temperature at which a uniform conductive polymer film can be obtained and is below the heat resistance temperature of the support, but is preferably in the range of room temperature to 300°C, more preferably in the range of room temperature to 250°C, and further preferably in the range of room temperature to 200°C.
[0120] The drying atmosphere may be any of air, inert gas, vacuum or reduced pressure. From the viewpoint of suppressing degradation of the polymer film, drying is preferably performed in an inert gas such as nitrogen or argon.
[0121] The thickness of the conductive polymer film obtained is not particularly limited, but is preferably within 10 -3 ~10 2 More preferably, 10 -3 ~10 -1 μm.
[0122] The conductive polymer film obtained from the conductive polymer composition of the present invention has excellent conductivity.
[0123] Furthermore, the conductive polymer film can be used as, for example, an electrode material, a transparent conductive film, and an electromagnetic wave shielding material.
[0124] Example
[0125] Related embodiments of the present invention are as follows.
[0126] It should be noted that the analytical instrument and the measurement method used in this example are as follows.
[0127] [GC measurement]
[0128] Device: Made by Shimadzu, GC-2014.
[0129] [NMR measurement]
[0130] Device: VARIAN, Gemini-200.
[0131] [Surface resistivity measurement]
[0132] Equipment: Loresta GP MCP-T600 manufactured by Mitsubishi Chemical Corporation, or Hiresta UXMCP-TH8000 manufactured by Mitsubishi Chemical Corporation
[0133] [Film thickness measurement]
[0134] Device: DEKTAK XT manufactured by BURKER.
[0135] [Viscosity measurement]
[0136] Device: Complete viscometer / BROOKFIELDVISCOMETER DV-1Prime.
[0137] [Total light transmittance]
[0138] Device: Haze Meter NDH 4000, manufactured by Nippon Denshoku Industries.
[0139] [Method for producing conductive film]
[0140] The conductive polymer composition prepared in the examples, etc. (for example, the above-mentioned polythiophene (A)) was applied to a polyester film (COSMOSHINE A4100 manufactured by Toyobo) using a wire bar coater to form a coating film having a wet film thickness of 12 μm. The film was then dried by heating at 150° C. for 5 minutes in the air to obtain a conductive polymer film.
[0141] [Method for producing conductive thick film]
[0142] 500 μL of a conductive polymer composition containing a conductive polymer (for example, the above-mentioned polythiophene (A)) prepared in Examples etc. was dropped onto a 25 mm square alkali-free glass plate using a microsyringe, and the plate was dried by heating at 120° C. for 60 minutes in air to obtain a conductive polymer film.
[0143] [Method for producing electromagnetic wave shielding material]
[0144] The conductive polymer composition prepared in the examples, etc. (e.g., the polythiophene (A) described above) was applied to a polyester film (COSMOSHINE A4100 manufactured by Toyobo) using a wire bar coater to form a coating film having a wet film thickness of 100 μm. The film was then dried by heating at 120° C. for 60 minutes in the air to obtain an electromagnetic wave shielding material.
[0145] [Electromagnetic wave shielding measurement]
[0146] The electromagnetic shielding material produced by the above production method was measured for electromagnetic shielding properties at 100 kHz to 1 GHz using a network analyzer according to the KEC method (a method for measuring electromagnetic shielding properties developed by the Kansai Electronic Industry Promotion Center).
[0147] [Method for producing a resistive film on the surface of an electromagnetic wave absorbing material]
[0148] The conductive polymer composition prepared in the examples, etc. (for example, the above-mentioned polythiophene (A)) is coated on a 50×100 mm square alkali-free glass plate using a wire bar coater, and then heated and dried at 200°C for 2 minutes in the atmosphere to obtain a resistive film for the surface of the electromagnetic wave absorbing material.
[0149] Example 1.
[0150] According to Synthesis Examples 1 and 2 of the known document (Japanese Patent Publication No. 2019-196443), a 1 wt% poly(3-[(2,3-dihydrothieno[3,4-b][1,4] ... An aqueous solution of PEDOT-MPS (a polymer composed of a structural unit represented by the following general formula (2) and a structural unit represented by the following general formula (3)). The PEDOT-MPS has a weight average molecular weight of 6303 in terms of standard polystyrene measured by gel permeation chromatography, and contains 44 ppm of iron ions and 12 ppm of sodium ions (to the polymer).
[0151]
[0152] In a glass container, 7.4 g of a methanol solution containing 5 wt% dioctylamine was added to 50.0 g of an aqueous solution containing 1 wt% of the above PEDOT-MPS while stirring, and the mixture was stirred at room temperature for 1 hour. The precipitate was separated into a solid and a liquid by a vacuum filter, and then the precipitate was vacuum dried to obtain 0.6 g of polythiophene A (solid). In addition, polythiophene A corresponds to the polythiophene (A) in which M is dioctylammonium, and its conductivity is 326 S / cm.
[0153] 0.1 g of the above-mentioned polythiophene A (solid) was dissolved in 9.9 g of isopropanol as an organic solvent (C), and 10 g of an isopropanol solution containing 1.0 wt% of polythiophene A was prepared. Then, 90 g of an isopropanol dispersion of 0.5 wt% silver nanowires (Sigma-Aldrich product number 739421, di am.×L=60 nm×10 μm) was added to the isopropanol solution as an organic solvent dispersible metal (B), and stirred and mixed. As a result, a conductive polymer composition having a solid content concentration of 0.10 wt% of polythiophene A and a solid content concentration of 0.45 wt% of silver nanowires was obtained. A conductive film was prepared using the obtained conductive polymer composition by the above method, and the surface resistance value was measured. The surface resistance value is shown in Table 1.
[0154] Example 2.
[0155] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 0.25 g of the polythiophene A (solid) was dissolved in 24.75 g of isopropanol as an organic solvent (C) to prepare 25 g of an isopropanol solution containing 1.0 wt% of polythiophene A. 75 g of an isopropanol dispersion of 0.5 wt% silver nanowires (Sigma-Aldrich product number 739421, diam.×L=60 nm×10 μm) was added to the 25 g isopropanol solution, and the mixture was stirred and mixed. As a result, a conductive polymer composition having a solid content concentration of 0.25 wt% of polythiophene A and a solid content concentration of 0.38 wt% of silver nanowires was obtained. A conductive film was prepared using the obtained conductive polymer composition by the above method, and the surface resistance value was measured. The surface resistance value is shown in Table 1.
[0156] Example 3.
[0157] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 0.5 g of the polythiophene A (solid) was dissolved in 49.5 g of isopropanol as an organic solvent (C) to prepare 50 g of an isopropanol solution containing 1.0 wt% of polythiophene A. 50 g of an isopropanol dispersion of 0.5 wt% silver nanowires (Sigma-Aldrich product number 739421, diam.×L=60 nm×10 μm) was added to the 50 g isopropanol solution, and the mixture was stirred and mixed. As a result, a conductive polymer composition having a solid content concentration of 0.5 wt% of polythiophene A and a solid content concentration of 0.25 wt% of silver nanowires was obtained. A conductive film was prepared using the obtained conductive polymer composition by the above method, and the surface resistance value was measured. The surface resistance value is shown in Table 1.
[0158] Example 4.
[0159] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 0.75 g of the polythiophene A (solid) was dissolved in 74.25 g of isopropanol as an organic solvent (C) to prepare 75 g of an isopropanol solution containing 1.0 wt% of polythiophene A. 25 g of an isopropanol dispersion of 0.5 wt% silver nanowires (Sigma-Aldrich product number 739421, diam.×L=60 nm×10 μm) was added to the 75 g isopropanol solution, and the mixture was stirred and mixed. As a result, a conductive polymer composition having a solid content concentration of 0.75 wt% of polythiophene A and a solid content concentration of 0.13 wt% of silver nanowires was obtained. A conductive film was prepared using the obtained conductive polymer composition by the above method, and the surface resistance value was measured. The surface resistance value is shown in Table 1.
[0160] Example 5.
[0161] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 0.1 g of the polythiophene A (solid) was dissolved in 9.9 g of isopropanol as an organic solvent (C) to prepare 10 g of an isopropanol solution containing 1.0 wt% of polythiophene A. 90 g of an isopropanol dispersion of 0.5 wt% silver nanowires (Sigma-Aldrich product number 778095, diam.×L=120-150 nm×20-50 μm) was added to the 10 g of the isopropanol solution and stirred and mixed. As a result, a conductive polymer composition having a solid content concentration of 0.1 wt% of polythiophene A and a solid content concentration of 0.45 wt% of silver nanowires was obtained. A conductive film was prepared using the obtained conductive polymer composition by the above method, and the surface resistance value was measured. The surface resistance value is shown in Table 1.
[0162] Comparative Example 1.
[0163] 99 g of a 0.5 wt% silver nanowire isopropanol dispersion (Sigma-Aldrich product number 739421, diam.×L=60 nm×10 μm) was stirred and mixed with 1 g of ethyl cellulose (Tokyo Chemical Industry product code E0265) which is a non-conductive resin. As a result, a composition having a solid content concentration of 1 wt% of ethyl cellulose and a solid content concentration of 0.495 wt% of silver nanowires was obtained. A conductive film was prepared using the above-mentioned method using the obtained composition, and the surface resistance value was measured. The surface resistance value is shown in Table 1.
[0164] Comparative Example 2.
[0165] 99.9 g of a 0.5 wt% silver nanowire isopropanol dispersion (Sigma-Aldrich product number 739421, diam.×L=60 nm×10 μm) was stirred and mixed with 0.1 g of ethyl cellulose (Tokyo Chemical Industry product code E0265) which is a non-conductive resin. As a result, a composition having a solid content concentration of 0.1 wt% of ethyl cellulose and a solid content concentration of 0.4995 wt% of silver nanowires was obtained. A conductive film was prepared using the above-mentioned method using the obtained composition, and the surface resistance value was measured. The surface resistance value is shown in Table 1.
[0166] Comparative Example 3.
[0167] 0.1 g of PEDOT:PSS particles (Sigma-Aldrich product number 768618) were added to 99.9 g of a 0.5 wt% silver nanowire isopropanol dispersion (Sigma-Aldrich product number 739421, diam.×L=60 nm×10 μm), and the mixture was stirred and mixed using a homogenizer, but the PEDOT:PSS particles were not dispersed, and silver precipitation occurred, and a uniform dispersion composition could not be obtained. In addition, the composition could not be formed into a film.
[0168] Comparative Example 4.
[0169] Since PEDOT:PSS and silver nanowires could not be mixed in Comparative Example 3, a PEDOT:PSS film was formed on the silver nanowire film.
[0170] First, a conductive film was prepared by the above-mentioned method using a 0.5 wt % isopropyl alcohol dispersion of silver nanowires (product number 739421 manufactured by Sigma-Aldrich, diam.×L=60 nm×10 μm).
[0171] Then, 84.9 g of PH500 (PEDOT:PSS dispersion aqueous solution manufactured by Hreaeus, solid content concentration 1.1 wt%), 10 g of ethylene glycol (product code 000-29335 manufactured by Kishida Chemicals), sorbitol (product code 198-03755 manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), and 0.1 g of OLFINE Exp.4200 (manufactured by Nissin Chemical Industries, Ltd.) were mixed and stirred to obtain a conductive polymer composition. The conductive polymer composition was repeatedly applied on the conductive film to prepare a conductive film by the above method. The surface resistance value of the obtained multilayer film was measured. The surface resistance value is shown in Table 1.
[0172] Reference Example 1.
[0173] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 0.1 g of the polythiophene A (solid) was dissolved in 9.9 g of isopropanol as an organic solvent (C) to prepare 10 g of an isopropanol solution containing 1.0 wt % of polythiophene A. A conductive film was prepared using the isopropanol solution by the above method, and the surface resistance value was measured. The surface resistance value is shown in Table 1.
[0174] Reference Example 2.
[0175] A conductive film was prepared by the above method using a 0.5 wt % silver nanowire isopropanol dispersion (Sigma-Aldrich product number 739421, diam.×L=60 nm×10 μm), and the surface resistance value was measured. The surface resistance value is shown in Table 1.
[0176] Reference Example 3.
[0177] PH500 (PEDOT:PSS dispersion aqueous solution manufactured by Hreaeus, solid content concentration 1.1 wt%) 84.9 g, ethylene glycol (Kishida Chemicals, product number 000-29335) 10 g, sorbitol (Fuji FIRM Wako Pure Chemicals, product number 198-03755) and OLFINE Exp.4200 (Nissin Chemical Industries, Ltd.) 0.1 g were stirred and mixed. As a result, a composition having a solid content concentration of 0.9 wt% of PEDOT:PSS was obtained. A conductive film was prepared by the above method using the obtained composition, and the surface resistance value was measured. The surface resistance value is shown in Table 1.
[0178] [Table 1]
[0179]
[0180] As shown in Table 1, the composition of the present invention comprising polythiophene (A), an organic solvent-dispersible metal (B) and an organic solvent (C) can provide a film having a low surface resistance value.
[0181] Furthermore, the conductive polymer composition of the present invention does not cause aggregation and is excellent in total light transmittance and storage stability, and therefore has particularly preferable and remarkable effects in industrial utilization.
[0182] Example 6.
[0183] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 0.25 g of the polythiophene A (solid) was dissolved in 24.75 g of ethanol as an organic solvent (C) to prepare 25 g of an ethanol solution containing 1.0 wt% of polythiophene A. 95 g of an ethanol dispersion of 0.5 wt% silver nanowires (product name T-AG219 manufactured by Starlight PMC) was added to 5 g of the ethanol solution and stirred and mixed. As a result, a conductive polymer composition having a solid content concentration of 0.05 wt% of polythiophene A and a solid content concentration of 0.48 wt% of silver nanowires was obtained. A conductive thick film was prepared using the obtained conductive polymer composition by the above method, and the surface resistance value was measured. The surface resistance value (initial surface resistance value) at this time is shown in Table 2. In addition, the surface resistance value (surface resistance value after the test) of the conductive thick film after being stored in the atmosphere at 85°C and 85% RH for 250 hours is shown in Table 2.
[0184] Example 7.
[0185] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 0.25 g of the polythiophene A (solid) was dissolved in 24.75 g of ethanol as an organic solvent (C) to adjust to 25 g of an ethanol solution containing 1.0 wt% polythiophene A. 92.5 g of an ethanol dispersion of 0.5 wt% silver nanowires (product name T-AG219 manufactured by Starlight PMC) was added to 7.5 g of the ethanol solution and stirred and mixed. As a result, a conductive polymer composition having a solid content concentration of 0.075 wt% of polythiophene A and a solid content concentration of 0.46 wt% of silver nanowires was obtained. A conductive thick film was prepared using the obtained conductive polymer composition by the above method, and the surface resistance value was measured. The surface resistance value (initial surface resistance value) at this time is shown in Table 2. In addition, the surface resistance value (surface resistance value after the test) of the conductive film after being stored in the atmosphere at 85°C and 85% RH for 250 hours is shown in Table 2.
[0186] Example 8.
[0187] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 0.25 g of the polythiophene A (solid) was dissolved in 24.75 g of ethanol as an organic solvent (C) to prepare 25 g of an ethanol solution containing 1.0 wt% polythiophene A. 90 g of an ethanol dispersion of 0.5 wt% silver nanowires (product name T-AG219 manufactured by Starlight PMC) was added to 10 g of the ethanol solution and stirred and mixed. As a result, a conductive polymer composition having a solid content concentration of 0.1 wt% of polythiophene A and a solid content concentration of 0.45 wt% of silver nanowires was obtained. A conductive thick film was prepared using the obtained conductive polymer composition by the above method, and the surface resistance value was measured. The surface resistance value (initial surface resistance value) at this time is shown in Table 2. In addition, the surface resistance value (surface resistance value after the test) of the conductive film after being stored in the atmosphere at 85°C and 85% RH for 250 hours is shown in Table 2.
[0188] Example 9.
[0189] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 1 g of the polythiophene A (solid) was dissolved in 99 g of ethanol as an organic solvent (C) to prepare 100 g of an ethanol solution containing 1.0 wt% polythiophene A. 40 g of an ethanol dispersion of 0.5 wt% silver nanowires (product name T-AG219 manufactured by Starlight PMC) was added to 60 g of the ethanol solution and stirred to mix. As a result, a conductive polymer composition having a solid content concentration of 0.6 wt% of polythiophene A and a solid content concentration of 0.2 wt% of silver nanowires was obtained. A conductive thick film was prepared using the obtained conductive polymer composition by the above method, and the surface resistance value was measured. The surface resistance value (initial surface resistance value) at this time is shown in Table 2. In addition, the surface resistance value (surface resistance value after the test) of the conductive film after being stored in the atmosphere at 85°C and 85% RH for 250 hours is shown in Table 2.
[0190] Example 10.
[0191] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 1 g of the polythiophene A (solid) was dissolved in 99 g of ethanol as an organic solvent (C) to prepare 100 g of an ethanol solution containing 1.0 wt% polythiophene A. 20 g of an ethanol dispersion of 0.5 wt% silver nanowires (product name T-AG219 manufactured by Starlight PMC) was added to 80 g of the ethanol solution and stirred to mix. As a result, a conductive polymer composition having a solid content concentration of 0.8 wt% of polythiophene A and a solid content concentration of 0.1 wt% of silver nanowires was obtained. A conductive thick film was prepared using the obtained conductive polymer composition by the above method, and the surface resistance value was measured. The surface resistance value (initial surface resistance value) at this time is shown in Table 2. In addition, the surface resistance value (surface resistance value after the test) of the conductive film after being stored in the atmosphere at 85°C and 85% RH for 250 hours is shown in Table 2.
[0192] Reference Example 4.
[0193] A conductive thick film was prepared by the above method using a 0.5 wt% silver nanowire ethanol dispersion (product name T-AG219 manufactured by Starlight PMC), and the surface resistance value was measured. The surface resistance value at this time (initial surface resistance value) is shown in Table 2. In addition, the surface resistance value of the conductive film after being stored in the atmosphere at 85°C and 85% RH for 250 hours (surface resistance value after the test) is shown in Table 2.
[0194] [Table 2]
[0195]
[0196] As shown in Table 2, the composition of the present invention comprising polythiophene (A), an organic solvent-dispersible metal (B) and an organic solvent (C) can provide a conductive film having high wet heat durability.
[0197] Example 11.
[0198] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 0.25 g of the polythiophene A (solid) was dissolved in 24.75 g of ethanol as an organic solvent (C) to prepare 25 g of an ethanol solution containing 1.0 wt% of polythiophene A. 95 g of an ethanol dispersion of 0.5 wt% silver nanowires (product name T-AG219 manufactured by Starlight PMC) was added to 5 g of the ethanol solution and stirred and mixed. As a result, a conductive polymer composition having a solid content concentration of 0.05 wt% of polythiophene A and a solid content concentration of 0.48 wt% of silver nanowires was obtained. A conductive thick film was prepared using the obtained conductive polymer composition by the above method, and the surface resistance value was measured. The surface resistance value at this time (initial surface resistance value) is shown in Table 3. In addition, the surface resistance value (surface resistance value after the test) after being stored in the atmosphere at 200°C for 1 hour is shown in Table 3.
[0199] Example 12.
[0200] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 0.25 g of the polythiophene A (solid) was dissolved in 24.75 g of ethanol as an organic solvent (C) to prepare 25 g of an ethanol solution containing 1.0 wt% polythiophene A. 90 g of an ethanol dispersion of 0.5 wt% silver nanowires (product name T-AG219 manufactured by Starlight PMC) was added to 10 g of the ethanol solution and stirred and mixed. As a result, a conductive polymer composition having a solid content concentration of 0.1 wt% of polythiophene A and a solid content concentration of 0.45 wt% of silver nanowires was obtained. A conductive thick film was prepared using the obtained conductive polymer composition by the above method, and the surface resistance value was measured. The surface resistance value at this time (initial surface resistance value) is shown in Table 3. In addition, the surface resistance value (surface resistance value after the test) after being stored in the atmosphere at 200°C for 1 hour is shown in Table 3.
[0201] Example 13.
[0202] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 1 g of the polythiophene A (solid) was dissolved in 99 g of ethanol as an organic solvent (C) to prepare 100 g of an ethanol solution containing 1.0 wt% polythiophene A. 40 g of an ethanol dispersion of 0.5 wt% silver nanowires (product name T-AG219 manufactured by Starlight PMC) was added to 60 g of the ethanol solution and stirred to mix. As a result, a conductive polymer composition having a solid content concentration of 0.6 wt% of polythiophene A and a solid content concentration of 0.2 wt% of silver nanowires was obtained. A conductive thick film was prepared using the obtained conductive polymer composition by the above method, and the surface resistance value was measured. The surface resistance value at this time (initial surface resistance value) is shown in Table 3. In addition, the surface resistance value (surface resistance value after the test) after being stored in the atmosphere at 200°C for 1 hour is shown in Table 3.
[0203] Reference Example 5.
[0204] A conductive thick film was prepared by the above method using a 0.5 wt% silver nanowire ethanol dispersion (product name T-AG219 manufactured by Starlight PMC), and the surface resistance value was measured. The surface resistance value at this time (initial surface resistance value) is shown in Table 3. In addition, the surface resistance value after storage at 200°C in the atmosphere for 1 hour (surface resistance value after the test) is shown in Table 3.
[0205] [Table 3]
[0206]
[0207] As shown in Table 3, the composition of the present invention comprising polythiophene (A), an organic solvent-dispersible metal (B) and an organic solvent (C) can provide a conductive film having high thermal stability.
[0208] Example 14.
[0209] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 1 g of the polythiophene A (solid) was dissolved in 99 g of ethanol as an organic solvent (C) to prepare 100 g of an ethanol solution containing 1.0 wt% polythiophene A. 20 g of an ethanol dispersion of 0.5 wt% silver nanowires (product name T-AG219 manufactured by Starlight PMC) was added to 80 g of the ethanol solution and stirred to mix. As a result, a conductive polymer composition having a solid content concentration of 0.8 wt% of polythiophene A and a solid content concentration of 0.1 wt% of silver nanowires was obtained. The obtained conductive polymer composition was used to prepare an electromagnetic wave shielding material by the above method, and the electromagnetic wave shielding properties were measured. The electromagnetic wave shielding properties are shown in Table 4.
[0210] Reference Example 6.
[0211] The same operation as in Example 1 was performed to obtain polythiophene A (solid), 0.8 g of which was dissolved in 99.2 g of ethanol as an organic solvent (C), and an electromagnetic wave shielding material was prepared by the above method using the ethanol solution containing 0.8 wt % of polythiophene A, and the electromagnetic wave shielding properties were measured. The electromagnetic wave shielding properties are shown in Table 4.
[0212] Reference Example 7.
[0213] 80 g of ethanol was added to 20 g of 0.5 wt% silver nanowire ethanol dispersion (product name T-AG219 manufactured by Starlight PMC) to prepare 100 g of 0.1 wt% silver nanowire ethanol dispersion. The obtained dispersion was used to prepare an electromagnetic wave shielding material by the above method, and the electromagnetic wave shielding properties were measured. The electromagnetic wave shielding properties are shown in Table 4.
[0214] [Table 3]
[0215]
[0216] As shown in Table 4, the composition of the present invention comprising polythiophene (A), an organic solvent-dispersible metal (B) and an organic solvent (C) can provide an excellent electromagnetic wave shielding film.
[0217] Example 15.
[0218] The same operation as in Example 1 was performed to obtain polythiophene A (solid), and 1 g of the polythiophene A (solid) was dissolved in 99 g of ethanol as an organic solvent (C) to prepare 100 g of an ethanol solution containing 1.0 wt% polythiophene A. 10 g of an ethanol dispersion of 0.5 wt% silver nanowires (product name T-AG219 manufactured by Starlight PMC) and 70 g of ethanol were added to 20 g of the ethanol solution and stirred and mixed. As a result, a conductive polymer composition having a solid content concentration of 0.2 wt% of polythiophene A and a solid content concentration of 0.05 wt% of silver nanowires was obtained. The obtained conductive polymer composition was applied to a wet film thickness of 12 μm by the above method, and dried to prepare a resistive film for the surface of an electromagnetic wave absorbing material. The surface resistance value and the total light transmittance are shown in Table 5.
[0219] Reference Example 8.
[0220] The same operation as in Example 1 was performed to obtain polythiophene A (solid), 1.0 g of the polythiophene A (solid) was dissolved in 99.0 g of ethanol as an organic solvent (C), and the ethanol solution containing 1.0 wt% of polythiophene A was applied by the above method to a wet film thickness of 46 μm, and dried to prepare a resistance film for the surface of an electromagnetic wave absorbing material. The surface resistance (Resistance) value and the total transmittance are shown in Table 5.
[0221] [Table 4]
[0222]
[0223] In order to absorb electromagnetic waves efficiently, impedance adjustment is applied to the surface of the electromagnetic wave absorber. Impedance adjustment means matching the surface impedance of the electromagnetic wave absorber with the impedance in the atmosphere (377Ω / □). That is, for the electromagnetic wave absorber, it is preferred to cover its surface with a resistance film with an impedance of 377Ω / □.
[0224] As shown in Table 5, the composition of the present invention comprising polythiophene (A), an organic solvent-dispersible metal (B) and an organic solvent (C) can provide a resistive film having a high total light transmittance (high transparency) for the surface of an electromagnetic wave absorbing material.
[0225] Industrial Applicability
[0226] The conductive polymer composition of the present invention forms a good conductive polymer film, exhibits high conductivity and excellent electromagnetic wave shielding effect, and therefore, it can be expected to be used in antistatic agents, solid electrolytes for capacitors, conductive coatings, electromagnetic wave shielding materials, electrochromic devices, electrode materials, thermoelectric conversion materials, transparent conductive films, chemical sensors or actuators, etc.
Claims
1. A conductive polymer composition comprising: Polythiophene (A) 0.01 to 10% by weight, 0.01 to 1.0 wt% of an organic solvent dispersible metal (B), and Organic solvent (C), The polythiophene (A) comprises at least one structural unit selected from the structural unit represented by the following general formula (1) and the structural unit represented by the following general formula (2), In the above general formulas (1) and (2), R 2 is a hydrogen atom, a methyl group, an ethyl group, a linear or branched alkyl group having 3 to 6 carbon atoms, or a fluorine atom; m is an integer of 1 to 10; n is 0 or 1; M + It represents an organic ammonium ion or a quaternary ammonium ion.
2. The conductive polymer composition according to claim 1, wherein The organic solvent dispersible metal (B) is at least one organic solvent dispersible metal selected from the group consisting of silver nanoparticles, silver nanoplates, silver nanowires, copper nanoparticles, copper nanoplates, and copper nanowires.
3. The conductive polymer composition according to claim 1, wherein The organic solvent dispersible metal (B) is organic solvent dispersible silver nanowires.
4. The conductive polymer composition according to claim 1, wherein The content of the polythiophene (A) is 0.1 to 5% by mass.
5. The conductive polymer composition according to claim 1, wherein The content of the organic solvent-dispersible metal (B) is 0.01 to 100 parts by mass relative to 1 part by mass of the polythiophene (A).
6. A film-making method, the method comprising: The conductive polymer composition according to any one of claims 1 to 5 is applied onto a support and then dried.
7. A film comprising: Polythiophene (A), and Organic solvent dispersible metal (B), The polythiophene (A) comprises at least one structural unit selected from the structural unit represented by the following general formula (1) and the structural unit represented by the following general formula (2), In the above general formulas (1) and (2), R 2 is a hydrogen atom, a methyl group, an ethyl group, a linear or branched alkyl group having 3 to 6 carbon atoms, or a fluorine atom; m is an integer of 1 to 10; n is 0 or 1; M + It represents an organic ammonium ion or a quaternary ammonium ion.