Method for removing xylene in neutral oil

Through the catalytic oxidation reaction of cobalt-manganese bimetallic catalyst, xylene in neutral oil is converted into carbon dioxide, solving the problem of difficult separation of xylene, achieving efficient and environmentally friendly removal effect, reducing recycling and treatment costs, and being suitable for Industrialized production.

CN118956443APending Publication Date: 2024-11-15XIAN THERMAL POWER RES INST CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411034093.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, xylene is difficult to separate in neutral oil collection, resulting in difficulty in recycling and disposal, which may cause harm to the ecological environment.

Method used

The cobalt-manganese bimetallic catalyst is used to convert xylene into carbon dioxide and water through a catalytic oxidation reaction, and the cobalt-manganese bimetallic catalyst is prepared by precipitation method, and catalytic oxidation treatment is carried out at a suitable temperature and oxygen environment.

Benefits of technology

Effectively remove xylene from neutral oil, reduces recycling and treatment costs, improves catalytic efficiency, and is easy to operate and achieves industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956443A_ABST
    Figure CN118956443A_ABST
Patent Text Reader

Abstract

The invention discloses a method for removing xylene in neutral oil, and belongs to the technical field of substance purification. The method comprises the following steps: adding cobalt-containing inorganic salt and manganese-containing inorganic salt into absolute ethyl alcohol, uniformly mixing to obtain a mixed solution, adding a precipitator into the mixed solution, uniformly mixing, collecting a precipitate after the reaction is completed, drying and calcining the precipitate, cooling, and grinding to obtain the cobalt-manganese bimetallic catalyst. The method comprises the following steps: heating a mixed solution of p-xylene and neutral oil to generate xylene steam, placing a cobalt-manganese bimetallic catalyst in an environment with preset oxygen purity, and introducing the xylene steam to remove the xylene steam through catalytic oxidation. The cobalt-manganese bimetallic catalyst is used to catalytically oxidize xylene into carbon dioxide and water, so that residual xylene in neutral oil is effectively removed, and the recovery and treatment cost of xylene is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material purification, and in particular to a method for removing xylene from neutral oil. Background Art

[0002] In the industrial field, neutral oil mainly comes with crude phenol produced from medium and low temperature coal tar. In crude phenol, the main substances include phenol, (o-, m-, p-) cresol, dimethylphenol and other phenol oil compounds, accounting for about 60-70% of crude phenol. These phenol oils are important raw materials for synthesizing triaryl phosphates; the remaining substances are non-phenol oil compounds such as benzene, indene, naphthalene, etc. These substances are collectively referred to as "neutral oils", which account for a small proportion in crude phenol. Neutral oil has a great influence on the deep processing of coal tar, and a certain process needs to be adopted to separate and remove it; at the same time, crude phenol also contains a small amount of pyridine and aniline alkaline impurities.

[0003] At present, the main process for separating neutral oil and purifying phenol oil in industry is alkali washing, which converts phenol oil into phenol salt that is easily soluble in water, and then uses distillation to separate the neutral oil. Finally, phenol salt is neutralized and reduced to crude phenol with sulfuric acid, and further distilled and purified to obtain the raw material for the production of triaryl phosphate. In the process of separating neutral oil, xylene is generally used for collection. The chemical formula of xylene is C8H 10 , is a mixture of three isomers with a certain polarity. Neutral oil can be well dissolved in xylene and thus separated from alkaline phenol salts.

[0004] However, xylene is a low-toxic chemical. It is difficult to separate xylene from the mixed solution after using xylene to collect neutral oil. Therefore, the recovery and disposal of the mixed solution is a major problem faced. Improper disposal will cause harm to the ecological environment. Summary of the invention

[0005] The invention provides a method for removing xylene from neutral oil in order to solve the problem of treating residual xylene in a mixed solution after neutral oil is collected by using xylene.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a method for removing xylene from neutral oil, comprising the following steps:

[0008] The cobalt-containing inorganic salt and the manganese-containing inorganic salt are added to anhydrous ethanol and mixed evenly to obtain a mixed solution, a precipitant is added to the mixed solution and mixed evenly, after the reaction is completed, a precipitate is collected, the precipitate is dried and calcined, and after cooling, the precipitate is ground to obtain a cobalt-manganese bimetallic catalyst;

[0009] A mixed solution of para-xylene and neutral oil is heated to generate xylene vapor. A cobalt-manganese bimetallic catalyst is placed in an environment of preset oxygen purity and the xylene vapor is introduced to remove the xylene vapor by catalytic oxidation.

[0010] The amount ratio of the cobalt-containing inorganic salt to the manganese-containing inorganic salt is 1:1 to 1:3; the amount of the precipitant added is 1 / 4 to 1 / 2 of the total amount of the cobalt-containing inorganic salt and the manganese-containing inorganic salt.

[0011] The precipitant is at least one of formic acid, acetic acid, oxalic acid and malonic acid.

[0012] The drying temperature is 60-80°C and the drying time is 12-24h.

[0013] The calcination temperature is 350-400°C, and the calcination time is 6-12h.

[0014] The mixed solution of p-xylene and neutral oil is heated by an oil bath or a metal bath.

[0015] The heating temperature of the mixed solution of p-xylene and neutral oil is 140-150°C.

[0016] The flow rate of xylene vapor is 50-150 mL / min.

[0017] The heating temperature during catalytic oxidation is 250-280°C.

[0018] The oxygen purity is not less than 99.5%.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention uses a cobalt-manganese bimetallic catalyst to catalytically oxidize xylene into carbon dioxide and water, effectively removes residual xylene in neutral oil, and reduces the recovery and treatment costs of xylene. The cobalt-manganese bimetallic catalyst used in the method is prepared by a precipitation method, which is simple to operate and easy to realize industrial production, and the added precipitant can be decomposed by drying and calcining treatment. After the precipitant is decomposed, more voids are formed, which increases the active sites of the catalyst and improves the catalytic effect of the cobalt-manganese bimetallic catalyst. In the catalytic oxidation process, sufficient oxygen and a suitable temperature are provided to activate the cobalt-manganese bimetallic catalyst, and the cobalt-manganese bimetallic catalyst can provide more oxygen vacancies, effectively improving the efficiency of catalytic oxidation. Through the detection of the gas chromatogram, it can be seen that there is only a characteristic peak of CO2 in the catalytic oxidation reaction process, indicating that the cobalt-manganese bimetallic catalyst has converted xylene into CO2; and after about 6 hours of catalytic oxidation, xylene has been completely converted into CO2. In general, the present invention provides an efficient and environmentally friendly method for removing xylene from neutral oil, and the method is easy to operate, the reaction conditions are mild, and industrial application can be realized. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the following briefly introduces the drawings required for use in the embodiment:

[0022] Figure 1 The gas chromatogram of the product after catalytic oxidation of xylene for 2 hours using a cobalt-manganese bimetallic catalyst in Example 1 of the present invention;

[0023] Figure 2 The gas chromatogram of the product after 6 hours of catalytic oxidation of xylene using a cobalt-manganese bimetallic catalyst in Example 1 of the present invention;

[0024] Figure 3 This is a gas chromatogram of the product after catalytic oxidation of xylene using a cobalt-manganese bimetallic catalyst for 7 hours in Example 1 of the present invention. DETAILED DESCRIPTION

[0025] The present invention will be further described below in conjunction with the accompanying drawings:

[0026] In order to solve the problem of xylene separation in neutral oil collection, the present invention proposes a method for removing xylene by catalytic oxidation of xylene using a cobalt-manganese bimetallic catalyst CoMn2O4.

[0027] The cobalt-manganese bimetallic catalyst (CoMn2O4) catalyzes the oxidation of xylene as follows: first, (o-, m-, p-) xylene is catalytically oxidized to (o-, m-, p-) methylbenzyl alcohol; 2+ and Mn 3+ The metal cations are reduced, and then the (o-, m-, p-)methylbenzyl alcohol is oxidized to (o-, m-, p-)methylbenzaldehyde and (o-, m-, p-)methylbenzoic acid. The oxidation continues, and the final oxidation products are CO2 and H2O.

[0028] CoMn2O4 is a typical ionic cubic crystal with a space group of Fd-3m (F is a face-centered lattice type, d is a slip plane, -3 is a three-fold rotational inversion symmetry, and m is a mirror symmetry), in which oxygen atoms are in a face-centered cubic close-packed structure. In the catalytic oxidation process, sufficient oxygen and high temperature are required to activate the cobalt-manganese bimetallic catalyst CoMn2O4. At the same time, in this process, the formation of oxygen vacancies is crucial. The oxygen atoms in the lattice are detached, resulting in oxygen deficiency, thereby forming vacancies. Then the vacancies of the missing oxygen atoms are quickly filled with external high-purity O2. The lower oxygen migration activation energy accelerates the breaking of the chemical bonds of the reactants, thereby continuing the catalytic oxidation reaction and obtaining the final oxidation product. The reaction formula for the catalytic oxidation of xylene by the cobalt-manganese bimetallic catalyst CoMn2O4 is shown below:

[0029]

[0030] The method for removing xylene from neutral oil provided by the present invention specifically comprises the following steps:

[0031] The preparation process of CoMn2O4 is as follows: take a certain mass of cobalt-containing inorganic salt and manganese-containing inorganic salt, completely dissolve the two inorganic salts in anhydrous ethanol under 60-80°C water bath and stirring conditions to obtain a mixed solution, then add a precipitant to the mixed solution, continue heating and stirring until completely dissolved, collect the bottom precipitate after the reaction is completed, repeatedly wash the precipitate with water for 3-5 times, place the washed precipitate in a 60-80°C oven to dry for 12-24 hours, place the dried product in a muffle furnace for calcination for 6-12 hours, control the calcination temperature to 350-400°C, wait for the calcined product to naturally cool to room temperature, obtain the cobalt-manganese bimetallic catalyst through tabletting and grinding, and then place it in a sealed bag for standby use.

[0032] The reaction process of xylene catalytic oxidation by CoMn2O4 can be realized in a fixed bed reactor, specifically: a mixed solution of neutral oil and xylene is placed in a two-necked flask, one of which is connected to the air compressor pipeline to provide compressed air with a stable flow rate, and the other is connected to a tubular heating furnace; the mixed solution of neutral oil and xylene is heated to convert the xylene liquid into xylene vapor, and the xylene vapor is carried by compressed air through the tubular furnace equipped with CoMn2O4 catalyst at the same flow rate, and the heating temperature of the tubular furnace is maintained at 250-280°C; at the same time, the tubular furnace is also connected to an oxygen gas source; the end of the tubular furnace is connected to a high-temperature resistant tee, one of which is connected to a gas chromatograph for analysis and detection of the output gas components, and the other is connected to an exhaust gas collector. The conversion rate is regularly evaluated during the reaction process, and when it is evaluated that CO2 is basically unchanged, it can be determined that xylene has been completely converted into CO2.

[0033] The present invention provides a cobalt-manganese bimetallic catalyst CoMn2O4, which can efficiently catalyze the oxidation of xylene and completely convert it into CO2 and H2O, thereby reducing the recovery and disposal costs of xylene.

[0034] Furthermore, the method for preparing CoMn2O4 is a precipitation method, which is simple to operate and easy to realize industrial production, and the precipitation method is easy to control the morphology of the bimetallic catalyst. The precipitant is at least one of formic acid, acetic acid, oxalic acid, and malonic acid. The selected precipitant can be decomposed in the subsequent drying and calcination process, and more voids are formed after decomposition, which increases the active sites of the catalyst and improves the catalytic effect of the catalyst.

[0035] The ratio of the amount of the cobalt-containing inorganic salt to the amount of the manganese-containing inorganic salt is 1:1 to 1:3; the amount of the precipitant added is 1 / 4 to 1 / 2 of the total amount of the cobalt-containing inorganic salt and the manganese-containing inorganic salt. The limitation of the amount of the cobalt-containing inorganic salt and the manganese-containing inorganic salt can regulate the microstructure of the cobalt-manganese bimetallic catalyst CoMn2O4 and improve the catalytic efficiency and stability.

[0036] Furthermore, the mixed solution of neutral oil and xylene is heated in an oil bath or a metal bath, and the temperature is controlled at 140-150°C. The use of an oil bath or a metal bath can provide a stable heating temperature and control the rate at which xylene liquid is converted into xylene vapor.

[0037] Furthermore, the flow rate of xylene vapor is 50-150 mL / min. If the flow rate of xylene vapor passing through the catalyst is less than 50 mL / min, the generated carbon dioxide will remain in the tubular furnace for a longer time, affecting the reaction efficiency. If the flow rate exceeds 150 mL / min, the xylene cannot be catalytically oxidized in time due to the excessively fast flow rate, resulting in incomplete removal of xylene.

[0038] Furthermore, the oxygen purity during the catalytic oxidation reaction is not less than 99.5%. Under the action of oxygen, the cobalt-manganese bimetallic catalyst can fully catalyze the oxidation of xylene. The high concentration of oxygen atmosphere can also control the direction of the catalytic oxidation reaction and reduce the occurrence of some side reactions.

[0039] The following examples are intended to explain the present invention and should not be construed as limiting the present invention. In the following examples, unless otherwise specified, all materials used can be obtained through common channels; and the test methods used are conventional methods in the art.

[0040] Example 1

[0041] Weigh 5.82g (about 0.02mol) of cobalt nitrate hexahydrate and 4.90g (about 0.02mol) of manganese acetate tetrahydrate, stir for 60min in a 60°C water bath, dissolve cobalt nitrate hexahydrate and manganese acetate tetrahydrate in 50mL of anhydrous ethanol solution, add 100mL of 0.20mol / L oxalic acid solution prepared in advance, continue stirring for 60min in a 60°C water bath, let stand for 6h after stirring, separate the precipitate and wash it with water 5 times, dry the washed precipitate in an oven at 80°C for 12h, and then place the dried product in a muffle furnace for calcination at a calcination temperature of 370°C for 6h. After the calcined product is naturally cooled to room temperature, the cobalt-manganese bimetallic catalyst is obtained by tabletting and grinding, with a mesh size of about 40, and then placed in a sealed bag for standby use.

[0042] About 50 mL of a mixed solution of neutral oil and xylene is placed in a 250 mL two-necked flask, one of the two-necked flask ports is connected to an air compressor pipeline, the compressed air flow rate is controlled to be 50 mL / min, and the other port is connected to a tubular furnace, 4 g of a cobalt-manganese bimetallic catalyst is placed in the tubular furnace, the two-necked flask containing the mixed solution of neutral oil and xylene is placed in a metal bath, the heating temperature of the metal bath is controlled to be 150° C., the xylene liquid is converted into xylene vapor, and under the action of compressed air, the xylene vapor enters the tubular furnace containing the cobalt-manganese bimetallic catalyst at the same flow rate, the heating temperature of the tubular furnace is maintained at 260° C., heating is continued, and at the same time, the tubular furnace is also connected to 99.999% high-purity oxygen; the three-way valve at the end of the tubular furnace is opened to allow the tail gas to flow into the gas chromatograph through a pipeline about 2 meters long for analysis and detection, and the rest of the tail gas flows into the tail gas collector.

[0043] like Figure 1 to Figure 3 As shown, the gas chromatograph shows that Figure 1 There is only a characteristic peak of CO2 on the gas chromatogram, indicating that the use of cobalt-manganese bimetallic catalyst CoMn2O4 can fully catalyze the oxidation of xylene in the mixed solution and convert it into CO2. During the catalytic oxidation process, after heating for 6 hours, Figure 2 The peak height of CO2 is Figure 1 The peak height after heating for 2 h is large. Figure 3 After heating for 7 hours, the peak height of CO2 remained basically unchanged, which shows that after 6 hours of catalytic oxidation, all xylene has been converted into CO2.

[0044] Example 2

[0045] Weigh 2.91g (about 0.01mol) of cobalt nitrate hexahydrate and 4.90g (about 0.02mol) of manganese acetate tetrahydrate, stir for 60min in a 60°C water bath, dissolve cobalt nitrate hexahydrate and manganese acetate tetrahydrate in 50mL of anhydrous ethanol solution, add 100mL of 0.10mol / L oxalic acid solution prepared in advance, continue stirring for 60min in a 60°C water bath, let stand for 7h after stirring, separate the precipitate and wash it with water 5 times, dry the washed precipitate in a 60°C oven for 24h, and then place the dried product in a muffle furnace for calcination at a calcination temperature of 400°C for 6h. After the calcined product is naturally cooled to room temperature, the cobalt-manganese bimetallic catalyst is obtained by tabletting and grinding, with a mesh size of about 40, and then placed in a sealed bag for standby use.

[0046] About 50 mL of a mixed solution of neutral oil and xylene is placed in a 250 mL two-necked flask, one of the two-necked flask ports is connected to an air compressor pipeline, the compressed air flow rate is controlled to be 80 mL / min, and the other port is connected to a tubular furnace, 4 g of a cobalt-manganese bimetallic catalyst is placed in the tubular furnace, the two-necked flask containing the mixed solution of neutral oil and xylene is placed in a metal bath, the heating temperature of the metal bath is controlled to be 140° C., the xylene liquid is converted into xylene vapor, and under the action of compressed air, the xylene vapor enters the tubular furnace containing the cobalt-manganese bimetallic catalyst at the same flow rate, the heating temperature of the tubular furnace is maintained at 280° C., heating is continued, and at the same time, the tubular furnace is also connected to 99.995% high-purity oxygen; the three-way valve at the end of the tubular furnace is opened to allow the tail gas to flow into the gas chromatograph through a pipeline of about 2 meters in length for analysis and detection, and the rest of the tail gas flows into the tail gas collector.

[0047] The composition of the produced gas was detected by gas chromatography, and no other components were found except CO2.

[0048] Example 3

[0049] Weigh 2.91g (about 0.01mol) of cobalt nitrate hexahydrate and 4.90g (about 0.02mol) of manganese acetate tetrahydrate, stir for 60min in a water bath at 80°C, dissolve cobalt nitrate hexahydrate and manganese acetate tetrahydrate in 50mL of anhydrous ethanol solution, add 50mL of 0.20mol / L oxalic acid solution prepared in advance, continue stirring for 60min in a water bath at 80°C, let stand for 6h after stirring, separate the precipitate and wash it with water 5 times, dry the washed precipitate in an oven at 80°C for 18h, and then place the dried product in a muffle furnace for calcination at a calcination temperature of 350°C for 12h. After the calcined product is naturally cooled to room temperature, the cobalt-manganese bimetallic catalyst is obtained by tabletting and grinding, with a mesh size of about 40, and then placed in a sealed bag for standby use.

[0050] About 50 mL of a mixed solution of neutral oil and xylene is placed in a 250 mL two-necked flask, one of the two-necked flask ports is connected to an air compressor pipeline, the compressed air flow rate is controlled to be 100 mL / min, and the other port is connected to a tubular furnace, 4 g of a cobalt-manganese bimetallic catalyst is placed in the tubular furnace, the two-necked flask containing the mixed solution of neutral oil and xylene is placed in a metal bath, the heating temperature of the metal bath is controlled to be 145° C., the xylene liquid is converted into xylene vapor, and under the action of compressed air, the xylene vapor enters the tubular furnace containing the cobalt-manganese bimetallic catalyst at the same flow rate, the heating temperature of the tubular furnace is maintained at 270° C., heating is continued, and at the same time, the tubular furnace is also connected to 99.999% high-purity oxygen; the three-way valve at the end of the tubular furnace is opened to allow the tail gas to flow into the gas chromatograph through a pipeline about 2 meters long for analysis and detection, and the rest of the tail gas flows into the tail gas collector.

[0051] The composition of the produced gas was detected by gas chromatography, and no other components were found except CO2.

[0052] Example 4

[0053] Weigh 5.82g (about 0.02mol) of cobalt nitrate hexahydrate and 7.35g (about 0.03mol) of manganese acetate tetrahydrate, stir for 60min in a 70°C water bath, dissolve cobalt nitrate hexahydrate and manganese acetate tetrahydrate in 50mL of anhydrous ethanol solution, add 100mL of 0.20mol / L oxalic acid solution prepared in advance, continue stirring for 60min in a 70°C water bath, let stand for 6h after stirring, separate the precipitate and wash it with water 5 times, dry the washed precipitate in a 70°C oven for 24h, and then place the dried product in a muffle furnace for calcination at a calcination temperature of 380°C for 10h. After the calcined product is naturally cooled to room temperature, the cobalt-manganese bimetallic catalyst is obtained by tabletting and grinding, with a mesh size of about 40, and then placed in a sealed bag for standby use.

[0054] About 50 mL of a mixed solution of neutral oil and xylene is placed in a 250 mL two-necked flask, one of the two-necked flask ports is connected to an air compressor pipeline, the compressed air flow rate is controlled to be 150 mL / min, and the other port is connected to a tubular furnace, 4 g of a cobalt-manganese bimetallic catalyst is placed in the tubular furnace, the two-necked flask containing the mixed solution of neutral oil and xylene is placed in a metal bath, the heating temperature of the metal bath is controlled to be 150° C., the xylene liquid is converted into xylene vapor, and under the action of compressed air, the xylene vapor enters the tubular furnace containing the cobalt-manganese bimetallic catalyst at the same flow rate, the heating temperature of the tubular furnace is maintained at 270° C., heating is continued, and at the same time, the tubular furnace is also connected to 99.999% high-purity oxygen; the three-way valve at the end of the tubular furnace is opened to allow the tail gas to flow into the gas chromatograph through a pipeline about 2 meters long for analysis and detection, and the rest of the tail gas flows into the tail gas collector.

[0055] The composition of the produced gas was detected by gas chromatography, and no other components were found except CO2.

[0056] Example 5

[0057] Weigh 5.82g (about 0.02mol) of cobalt nitrate hexahydrate and 7.35g (about 0.03mol) of manganese acetate tetrahydrate, stir for 60min in a 60°C water bath, dissolve cobalt nitrate hexahydrate and manganese acetate tetrahydrate in 50mL of anhydrous ethanol solution, add 100mL of 0.15mol / L oxalic acid solution prepared in advance, continue stirring for 60min in a 60°C water bath, let stand for 8h after stirring, separate the precipitate and wash it with water 3 times, dry the washed precipitate in a 60°C oven for 24h, and then place the dried product in a muffle furnace for calcination at a calcination temperature of 390°C for 12h. After the calcined product is naturally cooled to room temperature, the cobalt-manganese bimetallic catalyst is obtained by tabletting and grinding, with a mesh size of about 40, and then placed in a sealed bag for standby use.

[0058] About 50 mL of a mixed solution of neutral oil and xylene is placed in a 250 mL two-necked flask, one of the two-necked flask ports is connected to an air compressor pipeline, the compressed air flow rate is controlled to be 120 mL / min, and the other port is connected to a tubular furnace, 4 g of a cobalt-manganese bimetallic catalyst is placed in the tubular furnace, the two-necked flask containing the mixed solution of neutral oil and xylene is placed in a metal bath, the heating temperature of the metal bath is controlled to be 150° C., the xylene liquid is converted into xylene vapor, and under the action of compressed air, the xylene vapor enters the tubular furnace containing the cobalt-manganese bimetallic catalyst at the same flow rate, the heating temperature of the tubular furnace is maintained at 280° C., heating is continued, and at the same time, the tubular furnace is also connected to 99.95% high-purity oxygen; the three-way valve at the end of the tubular furnace is opened to allow the tail gas to flow into a gas chromatograph through a pipeline about 2 meters long for analysis and detection, and the rest of the tail gas flows into a tail gas collector.

[0059] The composition of the produced gas was detected by gas chromatography, and no other components were found except CO2.

[0060] Example 6

[0061] Weigh 5.82g (about 0.02mol) of cobalt nitrate hexahydrate and 4.90g (about 0.02mol) of manganese acetate tetrahydrate, stir for 60min in a 60°C water bath, dissolve cobalt nitrate hexahydrate and manganese acetate tetrahydrate in 50mL of anhydrous ethanol solution, add 100mL of 0.10mol / L acetic acid solution prepared in advance, continue stirring for 60min in a 60°C water bath, let stand for 10h after stirring, separate the precipitate and wash it with water 5 times, dry the washed precipitate in an oven at 80°C for 12h, and then place the dried product in a muffle furnace for calcination at a calcination temperature of 350°C for 6h. After the calcined product is naturally cooled to room temperature, the cobalt-manganese bimetallic catalyst is obtained by tabletting and grinding, with a mesh size of about 40, and then placed in a sealed bag for standby use.

[0062] About 50 mL of a mixed solution of neutral oil and xylene is placed in a 250 mL two-necked flask, one of the two-necked flask ports is connected to an air compressor pipeline, the compressed air flow rate is controlled to be 80 mL / min, and the other port is connected to a tubular furnace, 4 g of a cobalt-manganese bimetallic catalyst is placed in the tubular furnace, the two-necked flask containing the mixed solution of neutral oil and xylene is placed in a metal bath, the heating temperature of the metal bath is controlled to be 150° C., the xylene liquid is converted into xylene vapor, and under the action of compressed air, the xylene vapor enters the tubular furnace containing the cobalt-manganese bimetallic catalyst at the same flow rate, the heating temperature of the tubular furnace is maintained at 250° C., heating is continued, and at the same time, the tubular furnace is also connected to 99.995% high-purity oxygen; the three-way valve at the end of the tubular furnace is opened to allow the tail gas to flow into the gas chromatograph through a pipeline of about 2 meters in length for analysis and detection, and the rest of the tail gas flows into the tail gas collector.

[0063] The composition of the produced gas was detected by gas chromatography, and no other components were found except CO2.

[0064] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the same. Although the present invention has been described in detail with reference to the above embodiments, a person skilled in the art can still modify or make equivalent substitutions to the specific implementations of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention are within the scope of protection of the claims of the present invention to be approved.

Claims

1. A method for removing xylene from neutral oil, characterized in that: The following steps are involved: The cobalt-containing inorganic salt and the manganese-containing inorganic salt are added to anhydrous ethanol and mixed evenly to obtain a mixed solution, a precipitant is added to the mixed solution and mixed evenly, after the reaction is completed, a precipitate is collected, the precipitate is dried and calcined, and after cooling, the precipitate is ground to obtain a cobalt-manganese bimetallic catalyst; A mixed solution of para-xylene and neutral oil is heated to generate xylene vapor. A cobalt-manganese bimetallic catalyst is placed in an environment of preset oxygen purity and the xylene vapor is introduced to remove the xylene vapor by catalytic oxidation.

2. A method for removing xylene from neutral oil according to claim 1, characterized in that: The amount ratio of the cobalt-containing inorganic salt to the manganese-containing inorganic salt is 1:1 to 1:3; the amount of the precipitant added is 1 / 4 to 1 / 2 of the total amount of the cobalt-containing inorganic salt and the manganese-containing inorganic salt.

3. The method for removing xylene from neutral oil according to claim 1, characterized in that: The precipitant is at least one of formic acid, acetic acid, oxalic acid and malonic acid.

4. The method for removing xylene from neutral oil according to claim 1, characterized in that: The drying temperature is 60-80°C and the drying time is 12-24h.

5. The method for removing xylene from neutral oil according to claim 1, characterized in that: The calcination temperature is 350-400°C, and the calcination time is 6-12h.

6. The method for removing xylene from neutral oil according to claim 1, characterized in that: The mixed solution of p-xylene and neutral oil is heated by an oil bath or a metal bath.

7. The method for removing xylene from neutral oil according to claim 1, characterized in that: The heating temperature of the mixed solution of p-xylene and neutral oil is 140-150°C.

8. The method for removing xylene from neutral oil according to claim 1, characterized in that: The flow rate of xylene vapor is 50-150 mL / min.

9. The method for removing xylene from neutral oil according to claim 1, characterized in that: The heating temperature during catalytic oxidation is 250-280°C.

10. The method for removing xylene from neutral oil according to claim 1, characterized in that: The oxygen purity is not less than 99.5%.

Citation Information

Patent Citations

  • Composition solution and method for online real-time removal of xylene in indoor air

    CN112999846A