Manganese-doped cobaltosic oxide and preparation method thereof

By adopting the preparation method of manganese-doped cobalt tetroxide in lithium-ion batteries, the problems of battery capacity attenuation and high cost in lithium-ion batteries are solved, and the battery capacity maintenance and electrical performance are achieved, which is suitable for industrial promotion.

CN118993163APending Publication Date: 2024-11-22ANHUI HANRUI NEW MATERIALS CO LTD

Patent Information

Application Number
CN202411144329.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The commercial layered oxide positive electrode materials in existing lithium-ion batteries have irreversible transition metal ion migration and oxygen anion loss during the charging and discharging process, resulting in reduced battery capacity attenuation and cycle stability, and extremely low doping, resulting in electricity. Decreased performance and high cost.

Method used

Manganese-doped cobalt tetroxide and its preparation method are adopted to control seed nucleation and particle growth by introducing gas oxidizing agent into the alkaline base liquid, and to prepare manganese-doped cobalt hydroxyl oxide with good spherical shape, uniform particle size and high tap density , and the manganese-doped cobalt tetroxide was prepared by low-temperature roasting, so as to maintain battery capacity and reduce cost.

Benefits of technology

It realizes the maintenance of battery capacity and cost reduction, excellent electrical performance, guarantees circulation performance, and is simple and easy to control, which is suitable for industrial promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993163A_ABST
    Figure CN118993163A_ABST
Patent Text Reader

Abstract

The invention discloses a manganese-doped cobaltosic oxide preparation method, which comprises: S1, mixing pure water, an alkaline precipitating agent and a liquid oxidizing agent to form a base solution, continuously introducing a gas oxidizing agent, and maintaining the pH value of the base solution to be alkaline; s2, adding a manganese-doped metal cobalt salt complexing solution and an alkaline precipitator to carry out a co-precipitation reaction, and keeping the pH value of the precipitation reaction to be alkaline to obtain manganese-doped cobalt oxyhydroxide; and S3, filtering and washing the manganese-doped cobalt oxyhydroxide in the S2, and finally roasting to obtain a manganese-doped cobaltosic oxide product. The method is simple and easy to control, industrialization of the produced manganese-doped cobaltosic oxide has the effect of reducing cost, and industrial popularization is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of battery materials, and in particular to manganese-doped cobalt tetroxide and a preparation method thereof. Background Art

[0002] Lithium-ion batteries are now widely used in portable electronics and electric vehicles. As more lithium ions are extracted from the lattice, the structure of commercial layered oxide cathode materials is prone to irreversible transition metal ion migration and unstable oxygen anion loss, resulting in harmful structural phase changes and oxygen release behavior, leading to battery capacity decay and reduced cycle stability. It has long been believed that only about 50-60% of the Li in layered structures such as lithium cobalt oxide (LCO) can be reversibly deintercalated during charge and discharge, corresponding to a reversible capacity of 140-165 mAh / g.

[0003] CN103232075A discloses a method for preparing cobalt hydroxide oxide, which is to synthesize cobaltous hydroxide under nitrogen protection, and then oxidize the cobaltous hydroxide into cobalt hydroxide oxide by air; CN113788501A discloses a method for preparing cobalt hydroxide oxide, which is to use ammonia solution as a complexing agent, synthesize cobalt hydroxide oxide by coprecipitation of salt + alkali + ammonia + oxidizing gas, and then separate large particles by a cyclone to achieve the purpose of shrinking the particle size distribution. However, the amount of cobalt added in these two methods is large, and the cost is too high. Although CN117682566A discloses a method for preparing doped cobalt hydroxide oxide, the particle size of the product prepared is large, and no further research is done on the battery capacity.

[0004] With the development of technology, in order to pursue higher electrical performance and cost-effectiveness, more and more doped samples have come out. However, the doping amount in the products of the existing technology is extremely low, less than 1%, and the electrical performance drops drastically with the increase of the doping amount. Therefore, how to appropriately reduce the amount of precious metal cobalt, which is conducive to commercial cost savings and ensures excellent electrical performance, that is, to prepare high-performance and cost-effective precursors has become a top priority. Summary of the invention

[0005] In order to ensure that the capacitance of the electrode material remains unchanged and to solve the problem of excessively high cost of the electrode material, the present invention provides a manganese-doped cobalt oxide and a preparation method thereof. The method is simple to prepare and can be operated continuously. The cost of the prepared product is lower than that of undoped cobalt oxide, and the capacitance is slightly higher or equal to that of undoped cobalt oxide.

[0006] The technical solution adopted by the present invention is: a method for preparing manganese-doped cobalt oxide, comprising the following steps: S1: Pure water, alkaline precipitant and liquid oxidant are mixed to form a base liquid, and then the gas oxidant is continuously introduced to keep the pH value of the base liquid alkaline and the temperature 60-80°C. The volume ratio of pure water to hydrogen peroxide in the base liquid is 1:0.002-0.01; S2: adding a manganese-doped cobalt salt complex solution and an alkaline precipitant to carry out a coprecipitation reaction, maintaining the pH value of the precipitation reaction at an alkaline level, and obtaining manganese-doped cobalt hydroxide oxide; S3: filtering and washing the manganese-doped cobalt hydroxide oxide in S2, and finally roasting to obtain a manganese-doped cobalt tetroxide product.

[0007] This application controls the growth morphology of cobalt hydroxide oxide particles well by gradually controlling the system pH value, stirring speed, and slurry density during the seed nucleation and crystal growth stages, and obtains cobalt hydroxide oxide with good sphericity, uniform particle size, and high tap density. After sintering, it is made into cobalt tetroxide and cobalt-doped lithium cobalt oxide. The electrical properties are excellent through the buckle test. Compared with undoped cobalt hydroxide oxide, the battery capacity is not significantly reduced, and the cycle performance is guaranteed, achieving the purpose of cost reduction. After long-term exploration by the inventor, it is found that when a large amount of manganese is doped in cobalt tetroxide, the manganese-doped cobalt tetroxide prepared in accordance with the technical solution of this application has the effect of reducing costs and maintaining the battery capacity unchanged, while other doping elements do not have this effect.

[0008] Preferably, steps S1 and S2 are carried out in a reactor, and the reactor is connected to a recovery device for treating the mixed liquid overflowing after the reactor is full, and for secondary precipitation of the mother liquor to recover the manganese-doped cobalt hydroxide oxide in the mixed liquid.

[0009] During the preparation process, when continuous feeding is required, the reactor will be unable to continue operating due to being full. Adding a recovery device can not only discharge the mixed liquid overflowing after the reactor is full, but also reprecipitate the mixed liquid to recover the manganese-doped cobalt hydroxide in the mixed liquid.

[0010] Preferably, in step S1, the liquid oxidant is hydrogen peroxide, and the gaseous oxidant is one or more of air, oxygen and ozone, and the hourly flow rate of the gaseous oxidant is greater than the volume of the reactor.

[0011] In the present application, liquid oxidant is added to the base liquid to inhibit particle growth and increase the nucleation speed; and gas oxidant is continuously introduced during the reaction process, so that the process can prepare small particle products with high tap density, and the particle size range can be controlled within 4~6μm.

[0012] Preferably, the alkaline precipitant in steps S1 and S2 is sodium hydroxide or potassium hydroxide solution.

[0013] Preferably, the pH of the base solution in step S1 is 10.0-12.0.

[0014] Preferably, the manganese-doped cobalt salt complex solution in step S2 comprises a complexing agent, a cobalt salt and a manganese salt, wherein the cobalt salt is one of cobalt nitrate, cobalt chloride and cobalt sulfate, and the anions of the cobalt salt and the manganese salt participating in the reaction are the same.

[0015] Preferably, the complexing agent is disodium EDTA.

[0016] Preferably, the molar ratio of manganese salt, cobalt salt and complexing agent is 0.01-0.05:1:0.001-0.01.

[0017] Preferably, in step S2, the manganese-doped cobalt salt complex solution and the alkaline precipitant are added to the reaction kettle in parallel.

[0018] Preferably, the concentration of the manganese-doped cobalt salt complex solution entering the reactor is 80-135 g / L, and the flow rate of the alkaline precipitant entering the reactor is dynamically adjusted according to the pH value of the precipitation reaction in S2 to keep the pH value at 10.0-12.0.

[0019] Preferably, the reaction temperature in steps S1 and S2 is 60-80° C., and the particle size growth rate of cobalt oxyhydroxide is controlled to be 0.02-0.20 μm / h by adjusting the rotation speed and pH value.

[0020] The particle size growth rate is controlled within this range, which can suppress the particle growth rate, make the particles grow slowly and densely, and thus increase the tap density.

[0021] Preferably, the particle size growth rate of cobalt oxyhydroxide is controlled as follows: when the particle size of cobalt oxyhydroxide is 0-2.5 μm, the rotation speed is controlled at 600-800 prm and the pH is controlled at 11.0-12.0; when the particle size is 2.5-6.0 μm, the rotation speed is controlled at 400-600 prm and the pH is controlled at 10.0-11.0.

[0022] Preferably, the washing step in S3 is divided into water washing first, alkali washing and finally water washing again, wherein the washing liquid temperature is 50-90° C. and the sodium hydroxide concentration is 80-400 g / L.

[0023] Preferably, the drying temperature in S3 is 100-110°C, and the drying time is 8-12h; wherein the moisture content of the material after drying is ≤0.5%.

[0024] The present application also provides manganese-doped cobalt tetroxide prepared by the above preparation method.

[0025] Beneficial effects of the present invention: The invention introduces a gas oxidant into an alkaline base liquid to oxidize divalent cobalt in the particle nucleation stage into trivalent cobalt, that is, the original β-flaky cobalt hydroxide is changed into γ-coarse lath cobalt oxyhydroxide, thereby changing the particle stacking mode. A liquid oxidant is added into the base liquid to ensure sufficient oxidation in the initial stage, so that the system is partially changed from the cobalt oxyhydroxide into tricobalt tetroxide, thereby changing the particle surface morphology. Then, the manganese-doped tricobalt tetroxide with good sphericity, uniform particle size and high tap density is obtained through low-temperature calcination.

[0026] The present invention increases the solid content of particles in the reaction kettle by natural sedimentation through a connected recovery device, ensures long-term continuous synthesis, keeps the surface smooth, improves particle fluidity, increases the tap density of particles, reduces particle size distribution, and solves the problem of poor particle consistency.

[0027] The invention prepares manganese-doped cobalt hydroxide oxide and manganese-doped cobalt tetroxide with better sphericity and higher tap density by simultaneously doping manganese element. Not only is the preparation method simple and easy to control, but it also has the effect of reducing the cost of the industrialization of cobalt tetroxide, which is conducive to industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a scanning electron microscope image of the manganese-doped cobalt hydroxide oxide prepared in Example 1; Figure 2 This is a scanning electron microscope image of manganese-doped cobalt tetroxide prepared in Example 1; Figure 3 This is a scanning electron microscope image of cobalt oxyhydroxide prepared in Comparative Example 1; Figure 4 This is a scanning electron microscope image of cobalt tetroxide prepared in Comparative Example 1. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention more clear, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and a preferred implementation manner.

[0030] The following embodiments are all continuously reacted in a reactor, and the reactor is connected to a sedimentation tank. When the reactor is full, the mixed liquid in the reactor overflows into the sedimentation tank, and when the sedimentation tank is full, it overflows into the mother liquor tank. The slurry in the sedimentation tank naturally settles and circulates to the reactor to recover the overflowed manganese-doped cobalt hydroxide oxide. Example 1.

[0031] Prepare stock solution: 1. Mix cobalt sulfate, manganese sulfate and disodium EDTA with pure water, wherein the molar ratio of cobalt ions, manganese ions and disodium EDTA in the mixed solution is 1:0.03:0.001, and prepare a manganese-doped metal cobalt salt complex solution with a manganese and cobalt metal ion concentration of 120 g / L; 2. Mix sodium hydroxide and pure water to prepare a sodium hydroxide solution with a concentration of 160 g / L.

[0032] Preparation steps of manganese-doped cobalt tetroxide: S1. Use pure water, sodium hydroxide and hydrogen peroxide solution as the base liquid, stir the base liquid at a speed of 700 rpm, raise the temperature to 65°C, and continuously introduce air at a flow rate of 90 L / h; add sodium hydroxide solution with a concentration of 160 g / L to adjust the pH of the base liquid to 11.8; S2, adding manganese-doped cobalt salt complex solution and sodium hydroxide solution into the reactor at the same time for coprecipitation reaction, keeping the rotation speed and pH in step S1 unchanged; when the particle size grows to 2.0 μm, adjusting the rotation speed to 600 rpm, and adjusting the pH value of the reaction system to 10.7, until the precipitate particle size reaches 2.5 μm, obtaining seed solution 1; taking 1 / 2 of seed solution 1 for further synthesis, adjusting the rotation speed to 500 rpm, when the particle size reaches 4.3 μm, obtaining manganese-doped cobalt hydroxide oxide, the scanning electron microscope image is as shown in Figure 1 As shown; S3, the manganese-doped cobalt hydroxide oxide is filtered and washed, and then sintered in a rotary kiln at 700°C to finally obtain manganese-doped cobalt tetraoxide. The scanning electron microscope image is as follows: Figure 2 shown. Example 2.

[0033] Prepare stock solution: 1. Mix cobalt chloride, manganese sulfate and disodium EDTA with pure water, wherein the molar ratio of cobalt ions, manganese ions and disodium EDTA in the mixed solution is 1:0.05:0.005, and prepare a manganese-doped metal cobalt salt complex solution with a manganese and cobalt metal ion concentration of 80 g / L; 2. Mix sodium hydroxide and pure water to prepare a sodium hydroxide solution with a concentration of 320 g / L.

[0034] Preparation steps of manganese-doped cobalt tetroxide: S1. Use pure water, sodium hydroxide and hydrogen peroxide solution as the base liquid, stir the base liquid at a speed of 800 rpm, raise the temperature to 70°C, and continuously introduce air at a flow rate of 50 L / h; add sodium hydroxide solution with a concentration of 320 g / L to adjust the pH of the base liquid to 11.2; S2, adding manganese-doped cobalt salt complex solution and sodium hydroxide solution to the reactor at the same time for coprecipitation reaction, keeping the rotation speed and pH in step S1 unchanged; when the particle size grows to 2.5 μm, seed solution 1 is obtained, 1 / 2 of seed solution 1 is taken for further synthesis, the rotation speed is adjusted to 600 rpm, and the pH value of the reaction system is adjusted to 10.7, until the particle size of the precipitate reaches 4.0 μm, to obtain seed solution 2; 1 / 2 of seed solution 2 is taken for further synthesis, the rotation speed is adjusted to 500 rpm, and the pH value of the reaction system is adjusted to 10.5, and when the particle size reaches 6.0 μm, manganese-doped cobalt hydroxide oxide is obtained; S3, filtering and washing the manganese-doped cobalt hydroxide oxide, and then sintering it in a rotary kiln at 700° C. to finally obtain manganese-doped cobalt tetraoxide. Example 3.

[0035] Prepare stock solution: 1. Mix cobalt sulfate, manganese sulfate and disodium EDTA with pure water, wherein the molar ratio of cobalt ions, manganese ions and disodium EDTA in the mixed solution is 1:0.01:0.01, and prepare a manganese-doped metal cobalt salt complex solution with a manganese and cobalt metal ion concentration of 135 g / L; 2. Mix sodium hydroxide and pure water to prepare a sodium hydroxide solution with a concentration of 400 g / L.

[0036] Preparation steps of manganese-doped cobalt tetroxide: S1. Use pure water, sodium hydroxide and hydrogen peroxide solution as the base liquid, stir the base liquid at a speed of 750 rpm, raise the temperature to 75°C, and continuously introduce air at a flow rate of 80 L / h; add sodium hydroxide solution with a concentration of 400 g / L to adjust the pH of the base liquid to 11.0; S2, adding a manganese-doped cobalt salt complex solution and a sodium hydroxide solution to a reactor at the same time for a coprecipitation reaction, keeping the rotation speed and pH in step S1 unchanged; when the particle size grows to 2.5 μm, a seed solution 1 is obtained, 1 / 3 of the seed solution 1 is taken for further synthesis, the rotation speed is adjusted to 600 rpm, and the pH value of the reaction system is adjusted to 10.9, until the precipitated particle size reaches 4.5 μm, to obtain a seed solution 2; 1 / 3 of the seed solution 2 is taken for further synthesis, the rotation speed is adjusted to 550 rpm, and the pH value of the reaction system is adjusted to 10.6, and when the particle size reaches 6.0 μm, manganese-doped cobalt hydroxide oxide is obtained; S3, filtering and washing the manganese-doped cobalt hydroxide oxide, and then sintering it in a rotary kiln at 700° C. to finally obtain manganese-doped cobalt tetraoxide.

[0037] Comparative Example 1: Prepare stock solution: 1. Mix cobalt sulfate, disodium EDTA and pure water, the molar ratio of cobalt ions to disodium EDTA in the mixed solution is 1:0.003, and prepare a metal cobalt salt complex solution with a metal ion concentration of 120 g / L; 2. Mix sodium hydroxide and pure water to prepare a sodium hydroxide solution with a concentration of 160 g / L; Preparation steps of cobalt tetroxide: S1. Pure water, sodium hydroxide and hydrogen peroxide solution are used as base liquids, and the base liquid is stirred at a speed of 700 rpm, and the temperature is raised to 65°C. Air is continuously introduced at a flow rate of 60 L / h, and a sodium hydroxide solution with a concentration of 160 g / L is added to the reactor to adjust the pH of the base liquid to 10.8; S2. The metal cobalt salt complex solution and the sodium hydroxide solution are added to the reactor at the same time for coprecipitation reaction, and the speed and pH in step S1 are kept unchanged; when the particle size grows to 2.0 μm, the speed is adjusted to 600 rpm, and the pH value of the reaction system is adjusted to 10.7, until the particle size of the precipitate reaches 2.5 μm, to obtain a seed solution 1; 1 / 2 of the seed solution 1 is taken for continued synthesis, and the speed is adjusted to 500 rpm. When the particle size reaches 4.3 μm, cobalt hydroxide oxide is obtained, and the scanning electron microscope image is as shown in the figure Figure 3 As shown; S3, the cobalt hydroxide oxide is filtered and washed, and then sintered in a rotary kiln at 730°C to finally obtain cobalt tetroxide. The scanning electron microscope image is as follows: Figure 4 shown.

[0038] Battery performance test experiment 1. The final products in Example 1 and Comparative Example 1 were prepared into positive electrode materials in the following steps: Lithium carbonate and the manganese-doped cobalt oxide in Example 1 are mixed at a lithium to cobalt molar ratio of 1.05:1 and sintered; the sintering procedure includes a first sintering and a second sintering; the first sintering includes: setting a program temperature rise of 4-7°C / h, heating the material from room temperature to 800°C-1000°C, keeping it warm for 10 hours, then heating it to 960°C-1180°C, keeping it warm for 10 hours, and then cooling; the second sintering includes: heating the material obtained by the first sintering from room temperature to 850°C-1000°C, keeping it warm for 12 hours, and then cooling to obtain the positive electrode material of Example 1.

[0039] Lithium carbonate and the cobalt oxide in comparative example 1 are mixed according to a lithium to cobalt molar ratio of 1.05:1 and sintered; the sintering procedure includes a first sintering and a second sintering; the first sintering includes: setting a program temperature rise of 4-7°C / h, heating the material from room temperature to 800°C-1000°C, keeping it warm for 10 hours, then heating it to 960°C-1180°C, keeping it warm for 10 hours, and then cooling; the second sintering includes: heating the material obtained by the first sintering from room temperature to 850°C-1000°C, keeping it warm for 12 hours, and then cooling to obtain the positive electrode material of comparative example 1.

[0040] 2.Battery performance test: The positive electrode materials prepared in Example 1 and Comparative Example 1 were dissolved in NMP solvent with a mass ratio of 90:5:5 under vacuum to prepare a positive electrode slurry with a weight solid content of 80%, and then the positive electrode discs were prepared by coating, drying and punching. Then, a lithium battery was prepared in the order of positive electrode shell-positive electrode sheet-diaphragm-negative electrode sheet-stainless steel sheet-spring sheet-negative electrode shell, the electrolyte was 1 mol / L LiPF6 / EC:DMC (volume ratio of 1:1) with 10% (volume fraction) fluoroethylene carbonate (FEC), and the diaphragm was a polypropylene microporous membrane, and the lithium batteries of Example 1 and Comparative Example 1 were prepared respectively, and the battery performance is shown in Table 1.

[0041] Table 1 is the product electrical performance test data

[0042] It can be seen from the electron microscope image and the data in Table 1 that the cobalt hydroxide oxide and cobalt trioxide prepared in Example 1 have good sphericity, uniform particle size, and a tap density higher than that of Comparative Example 1; it indicates that the tap density and sphericity of Example 1 can be improved by doping with manganese element, continuously increasing the slurry density in the reactor, adjusting the stirring speed and the pH environment of the slurry, and appropriately selecting the number of seed crystals according to the particle size growth trend; the manganese-doped cobalt hydroxide oxide prepared in the present application is sintered into cobalt trioxide and cobalt-doped lithium cobaltate, and the electrical properties are excellent through the buckle test. Compared with undoped cobalt hydroxide oxide, the battery capacity is not significantly reduced, and the cycle performance is guaranteed.

[0043] The above descriptions are merely preferred embodiments and comparative examples of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing manganese-doped cobalt oxide, characterized in that: The steps include: S1: Pure water, alkaline precipitant and liquid oxidant are mixed to form a base liquid, and then a gas oxidant is continuously introduced to keep the pH value of the base liquid alkaline; S2: adding a manganese-doped cobalt salt complex solution and an alkaline precipitant to carry out a coprecipitation reaction, maintaining the pH value of the precipitation reaction at an alkaline level, and obtaining manganese-doped cobalt hydroxide oxide; S3: filtering and washing the manganese-doped cobalt hydroxide oxide in S2, and finally roasting to obtain a manganese-doped cobalt tetroxide product.

2. The preparation method according to claim 1, characterized in that: In step S1, the liquid oxidant is hydrogen peroxide; the gaseous oxidant is one or more of air, oxygen and ozone, and the hourly flow rate of the gaseous oxidant is greater than the volume of the reactor.

3. The preparation method according to claim 1, characterized in that: In steps S1 and S2, the alkaline precipitant is sodium hydroxide or potassium hydroxide solution.

4. The preparation method according to claim 1, characterized in that: In step S2, the manganese-doped cobalt salt complex solution comprises a complexing agent, a cobalt salt and a manganese salt, wherein the cobalt salt is one of cobalt nitrate, cobalt chloride and cobalt sulfate, and the anions of the cobalt salt and the manganese salt involved in the reaction are the same.

5. The preparation method according to claim 4, characterized in that: The complexing agent is disodium EDTA.

6. The preparation method according to claim 4, characterized in that: The molar ratio of the manganese salt, the cobalt salt and the complexing agent is 0.01-0.05:1:0.001-0.

01.

7. The preparation method according to claim 1, characterized in that: The concentration of the manganese-doped cobalt salt complex solution entering the reactor is 80~135 g / L, and the pH value of the coprecipitation reaction is maintained at 10.0~12.

0.

8. The preparation method according to claim 1, characterized in that: The reaction temperature in steps S1 and S2 is 60-80° C., and the particle size growth rate of cobalt oxyhydroxide is controlled to be 0.02-0.20 μm / h by adjusting the rotation speed and pH value.

9. The preparation method according to claim 8, characterized in that: The particle size growth rate of cobalt oxyhydroxide is controlled as follows: when the particle size of cobalt oxyhydroxide is 0-2.5 μm, the rotation speed is controlled at 600-800 prm and the pH is controlled at 11.0-12.0; when the particle size is 2.5-6.0 μm, the rotation speed is controlled at 400-600 prm and the pH is controlled at 10.0-11.

0.

10. A manganese-doped cobalt oxide, characterized in that: The manganese-doped cobalt oxide product is prepared by any preparation method of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method for large-grained spherical cobalt oxyhydroxide

    CN103232075A

  • Method for preparing hydroxyl cobalt oxide

    CN113788501A

  • Doped hydroxyl cobalt oxide and preparation method thereof

    CN117682566A

Cited By

  • Spherical cobaltosic oxide as well as preparation method and application thereof

    CN120622551A