Process for manufacture of lithium salts of bis (fluorosulfonyl) imides in solid form
The solvent is removed from the LiFSI solution through supercritical fluid extraction technology, which solves the problem of complexity in the preparation of solid form of LiFSI in the prior art, and achieves efficient and environmentally friendly high-purity LiFSI preparation, which is suitable for battery electrolytes.
Patent Information
- Application Number
- CN202380035031.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-21
- Filing Date
- 2023-04-12
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The steps for preparing lithium bis(fluorosulfonyl)imide (LiFSI) solid form in the prior art are complex, especially when the residual solvent amount is required as low as possible, and it is difficult to meet the requirements of battery electrolytes.
The supercritical fluid extraction method is used to contact the supercritical fluid from the solution containing LiFSI and solvent, and most of the solvent is removed, thereby recovering LiFSI in solid form.
It realizes simple equipment and reaction conditions, high yield and high purity LiFSI preparation, suitable for battery electrolytes, and is environmentally friendly.
Smart Images

Figure CN119053549A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority from the prior European patent application No. 22305583.1 filed on April 21, 2022, the entire contents of which are incorporated herein by reference for all purposes. Technical Field
[0003] The present invention relates to a method for preparing a lithium salt of bis(fluorosulfonyl)imide (LiFSI) in solid form. The present invention also relates to the solid LiFSI obtained therefrom and the use of such LiFSI in an electrolyte for a battery. Background Art
[0004] Bis(fluorosulfonyl)imide and its salts, in particular the lithium salt of bis(fluorosulfonyl)imide (LiFSI), are useful compounds in various technical fields, including in battery electrolytes.
[0005] The production of LiFSI is described in the literature. Of the different techniques described, most use a fluorination reaction with a fluorinating agent in a solvent.
[0006] For example, WO 2017 / 090877 (in the name of CLS) describes a method for producing LiFSI, which comprises the following steps: (1) reacting bis(chlorosulfonyl)imide with a fluorinating agent in a solvent and then treating with an alkaline agent to produce ammonium bis(fluorosulfonyl)imide; and (2) reacting ammonium bis(fluorosulfonyl)imide with a lithium-based substance. The solvent used in step (1) is selected from the group consisting of: alkyl ketones including acetone, methyl ethyl ketone and methyl isopropyl ketone; alcohols including methanol, anhydrous ethanol, 1-propanol and isopropanol; alkyl nitriles including acetonitrile and propionitrile; and ethers including tetrahydrofuran and dialkoxyalkanes. The solvent is then removed by distillation and concentrated under reduced pressure.
[0007] WO 2012 / 117961 (in the name of Nippon Soda) describes a process for producing fluorosulfonyl imide salts. According to Examples 1 and 2, ammonium di(fluorosulfonyl)imide is prepared from di(chlorosulfonyl)imide in acetonitrile. The solvent is then removed by distillation under reduced pressure.
[0008] JP 2016145147 (in the name of Nippon Shokubai) relates to a method for providing a fluorosulfonyl imide compound represented by formula (1), which is carried out by reacting a compound represented by formula (2) and 1 to 3 equivalents of a compound represented by composition formula (3) in a stoichiometric amount based on 1 mol of the compound in the presence of a solvent in an amount of 0 to 4 times the mass of the compound:
[0009]
[0010] NH4F(HF) p (3)
[0011] Where R 1 It is C 1-6 Fluoroalkyl, R 6 Is halogen or C 1-6 Fluoroalkyl, Cat1 + and Cat2 + is a monovalent group, and p is an integer of 1 to 10.
[0012] JP 2014201453 (in the name of Nippon Shokubai Co., Ltd.) describes a method for producing an alkali metal salt of a fluorosulfonyl imide, the method comprising the steps of synthesizing an alkali metal salt of a fluorosulfonyl imide in the presence of a reaction solvent, the reaction solvent containing at least one solvent selected from the group consisting of: a carbonate-based solvent, an aliphatic ether-based solvent, an ester-based solvent, an amide-based solvent, a nitro-based solvent, a sulfur-based solvent and a nitrile-based solvent, and subsequently concentrating the alkali metal salt solution of the fluorosulfonyl imide by distilling off the reaction solvent in the coexistence of the reaction solvent and at least one poor solvent for the alkali metal salt of the fluorosulfonyl imide, the poor solvent being selected from the group consisting of: an aromatic hydrocarbon-based solvent, an aliphatic hydrocarbon-based solvent and an aromatic ether-based solvent, the concentrating step comprising the step of mixing the above-mentioned poor solvent with a reaction solution containing the reaction solvent and the alkali metal salt of the fluorosulfonyl imide.
[0013] Supercritical fluid extraction has been used for recycling purposes. Notably, US 2003 / 0186110 (in the name of ECO BATINDIANA LLC, ONTO TECH LLC), CN 105406146 (in the name of HARBIN INST TECHNOLOGY), and CN 110534835 (in the name of University of Changzhou) disclose a method for removing electrolyte from energy storage devices (e.g., lithium batteries) using supercritical fluids.
[0014] Supercritical fluid extraction for extracting bis(fluorosulfonyl)imide (HFSI) from a reaction mixture containing an acid has also been described. Notably, WO 2021 / 082450 (in the name of GUANGZHOU LIWENTECH CO LTD) discloses a method for purifying HFSI from a reaction mixture containing a strong acid (e.g., concentrated sulfuric acid, phosphoric acid) and a FSI salt (e.g., NaFSI, KFSI or LiFSI, etc.) using supercritical extraction (particularly supercritical CO2 fluid). In addition, CN 111517293 (in the name of SHANGHAI INST ORGANICCHEMISTRY CAS, Chinese Academy of Sciences) describes a method for preparing HFSI using a supercritical fluid, the method comprising the following steps:
[0015]
[0016] Where X is an alkali metal; R 1 and R 2 and C1-12 alkyl substituted with F or all-F. Summary of the invention
[0017] As described in the literature, LIFSI is produced by fluorination in a solvent, such as an organic solvent, to disperse the reactive entities and react them.
[0018] However, such solvents need to be removed after the reaction to obtain products that are as pure as possible for battery applications.
[0019] The Applicant has realised that the steps for preparing LiFSI in solid form based on LiFSI in solution are complicated, especially when the amount of residual solvent has to be as low as possible in order to be well suited for battery electrolytes.
[0020] The Applicant was therefore faced with the problem of developing a new process for producing LiFSI which allows overcoming the complexity of the processes known to date.
[0021] Unexpectedly, the applicant has developed a method for producing LiFSI which is simple to perform in terms of equipment and reaction conditions and is very friendly from an environmental point of view.
[0022] Furthermore, the process of the invention allows obtaining LiFSI in solid form with very high yield and high purity, so that it can then be used in battery electrolyte solutions.
[0023] An advantageous process according to the invention for preparing LiFSI in solid form is based on supercritical fluid extraction.
[0024] Therefore, a first object of the present invention relates to a process for preparing LiFSI in solid form from a solution comprising at least one solvent and a LiFSI salt, which process is based on the use of a supercritical fluid. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Scheme representing the laboratory setup used in Example 2. DETAILED DESCRIPTION
[0026] In this application:
[0027] - the expression "comprising between ... and ..." is to be understood as including the limit values;
[0028] - any description (even those relating to a specific embodiment) is applicable to and interchangeable with other embodiments of the invention;
[0029] - When an element or component is said to be included in and / or selected from a list of listed elements or components, it should be understood that in the relevant embodiments explicitly considered herein, the element or component may also be any of these listed independent elements or components, or may also be selected from a group consisting of any two or more of the explicitly listed elements or components; any element or component listed in the list of elements or components may be omitted from this list; and
[0030] - Any recitation of numerical ranges by endpoints herein includes all numbers subsumed within the recited range as well as the endpoints of that range and equivalents thereof.
[0031] A first object of the present invention relates to a method for preparing a lithium salt of bis(fluorosulfonyl)imide (LiFSI) in solid form, the method comprising the following steps:
[0032] a) providing a solution comprising LiFSI and at least one solvent [LiFSI solution];
[0033] b) contacting the LiFSI solution with at least one supercritical fluid; and
[0034] c) recovering LiFSI in solid form.
[0035] The term "contacting" as used herein means that a solution is contacted with at least one supercritical fluid under specific pressure and temperature conditions, such as in a container, for a period of time sufficient for the fluid to remove at least a portion of the solvent present in the solution, preferably greater than 80.0%, greater than 90.0%, greater than 95.0%, greater than 99.0%, greater than 99.5% or even greater than 99.9% of the solvent.
[0036] The term "recovery" herein means removing or extracting LiFSI in solid form from the container in which step b) takes place.
[0037] The expression "supercritical fluid" means herein a gas (or a mixture of at least two gases) in its supercritical state. Depending on the gas used in step b), the pressure and temperature used in the container in which the contact between the solution and the supercritical fluid occurs are appropriately selected. More specifically, the gas used in step b) is maintained at or above its critical temperature and critical pressure in order to be in a supercritical state.
[0038] The term "container" herein means a container that is well suited for the process of the present invention, that is, adapted to withstand the pressures and temperatures used in the process of the present invention, as well as the possible corrosive properties of the reactants and products involved in the process. As described in detail below, the container used in this article can notably be an extraction column (also called a "column") or an autoclave.
[0039] According to the method of the present invention, at least one supercritical fluid is used to extract the LiFSI salt from the solution, which has several advantages. Supercritical fluids, such as sCO2, have obvious advantages and are generally readily available, cheap, non-toxic, non-explosive, and not organic solvents. In addition, the method of the present invention operates at moderate temperatures (less than 100°C), which ensures gentle handling of the LiFSI product. The method of the present invention also allows easy separation of one or more solvents and solid form extracts.
[0040] Preferably, step a) is performed batchwise, semi-continuously or continuously.
[0041] As disclosed above, the LiFSI solution comprises at least one solvent. Preferably, the LiFSI solution comprises one solvent. Alternatively, the LiFSI solution comprises two or more solvents, such as a mixture of two or three solvents.
[0042] Preferably, the solvent is selected from the group consisting of ethylene carbonate, propylene carbonate, butylene carbonate, γ-butyrolactone, γ-valerolactone, dimethoxymethane, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxane, 4-methyl-1,3-dioxolane, methyl formate, methyl acetate, methyl propionate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, sulfolane, 3-methylsulfolane, dimethyl sulfoxide, N,N-dimethylformamide, N-methyloxazolidinone, acetonitrile, valeronitrile, benzonitrile, ethyl acetate, isopropyl acetate, n-butyl acetate, nitromethane, nitrobenzene, trifluoroethanol, and mixtures thereof.
[0043] Preferred solvents include ethylene carbonate, propylene carbonate, butylene carbonate, tetrahydrofuran, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethyl acetate, isopropyl acetate and n-butyl acetate. Even more preferred solvents include dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethyl acetate, isopropyl acetate and n-butyl acetate. Still more preferred solvents include ethyl methyl carbonate and n-butyl acetate. The most preferred solvent is ethyl methyl carbonate.
[0044] In some embodiments, the LiFSI solution includes between 5 and 70 wt. % LiFSI based on the total weight of the LiFSI solution.
[0045] The LiFSI solution preferably contains between 10 and 60 wt.%, such as between 15 and 50 wt.%, between 20 and 40 wt.%, or between 25 and 35 wt.% LiFSI. As an example, the solution contains 30±2 wt.% LiFSI based on the total weight of the LiFSI solution.
[0046] The weight ratio of supercritical fluid / LiFSI solution used in the method of the present invention may vary between 1 / 1 and 4000 / 1. For example, the weight ratio of supercritical fluid / LiFSI solution preferably varies between 10 / 1 and 3500 / 1.
[0047] It will be clear to a person skilled in the art that the parameters of the process according to the invention may be appropriately selected and optimized based on, for example, the starting materials (particularly based on the purity of the product), and the scale on which the process is carried out, e.g. whether the process is carried out on an industrial scale or on a laboratory scale.
[0048] Preferably, step b) is carried out in a vessel at a pressure P of at least 73 bar (7.3 MPa).
[0049] Preferably, step b) is carried out at a temperature T between 30°C and 90°C.
[0050] Step b) may preferably be carried out in a vessel capable of withstanding high pressure.
[0051] According to this embodiment, step b) comprises contacting the solution of step a) with at least one supercritical fluid in a container.
[0052] A particular advantage of the process of the present invention is the short contact time in step b). Furthermore, advantageously, the contact time in step b) can be appropriately selected, for example based on the starting material and the desired yield.
[0053] Preferably, the contact time in step b) varies between a few seconds (e.g. 5 seconds) and 24 hours. More preferably, the contact time in step d) varies between 1 minute and 12 hours, such as between 5 minutes and 10 hours or between 10 minutes and 5 hours.
[0054] Preferably, step b) is performed by injecting a supercritical fluid at the bottom of the container. Advantageously, this allows improved mixing of the LiFSI solution with the supercritical fluid.
[0055] Preferably, during step b), the LiFSI solution is brought into contact with a fluid in a supercritical state.
[0056] Preferably, during step b), the LiFSI solution is contacted with two or more fluids in a supercritical state. The two or more fluids may be mixed, or may be contacted with the solution in sequence. As an example, the LiFSI solution may be contacted with a mixture of at least two supercritical fluids.
[0057] Furthermore, according to the present invention, at least one other component (also referred to herein as a modifier) may be mixed into the one or more supercritical fluids.
[0058] Advantageously, the at least one other component is chosen from polar solvents having a solubility in the supercritical fluid of less than 10 wt. %, based on the total weight of the supercritical fluid and the one or more other components.
[0059] More preferably, when the at least one other component is used, the amount thereof is in the range of 0.1 to 10 wt.%, such as 0.5 to 8 wt.% or 1 to 6 wt.%, based on the total weight of the supercritical fluid and the one or more other components.
[0060] Preferably, the at least one other component is selected from polar solvents, more preferably, from the group comprising alcohols, toluene, dimethyl sulfoxide (DMSO), acetonitrile, etc. According to a preferred embodiment, the polar solvent is an alcohol. Even more preferably, the alcohol is ethanol.
[0061] According to the invention, step b) can be repeated once or more than once.
[0062] For example, the method according to the present invention comprises a first step b) and a second step b'), wherein the same or different supercritical fluids or a mixture of at least two supercritical fluids are used in each of said step b) and said step b').
[0063] In some embodiments, the vessel used to contact the LiFSI solution with the at least one supercritical fluid in step b) is preferably at a pressure P of at least 73 bar (7.3 MPa).
[0064] In some embodiments, it is preferred that the vessel used to contact the LiFSI solution with the at least one supercritical fluid in step b) is at a temperature T between 30°C and 90°C during extraction.
[0065] Preferably, the temperature T in the container may vary between 37°C and 75°C, for example between 38°C and 70°C or between 40°C and 65°C.
[0066] Preferably, the pressure P in the container may be at least 80 bar (8.0 MPa), at least 100 bar (10.0 MPa), at least 130 bar (13.0 MPa) or at least 150 bar (15.0 MPa). Very high pressures may also be used in the method of the invention. For example, the pressure P in the container may be up to 200 bar (20.0 MPa) or 300 bar (30.0 MPa). The pressure in the container will typically be less than 500 bar (50.0 MPa), for example less than 450 bar (45.0 MPa), less than 400 bar (40.0 MPa) or even less than 350 bar (35.0 MPa).
[0067] According to an embodiment, step b) is performed by injecting the LiFSI solution into the pressurized container. The LiFSI solution can be injected into the container, for example, through a syringe or an inlet valve installed on the container.
[0068] According to another embodiment, step b) comprises:
[0069] b1) introducing the LiFSI solution into a container;
[0070] b2) pressurizing the container to a pressure of P;
[0071] b3) heating the container to a temperature T; and
[0072] b4) introducing at least one supercritical fluid into the container.
[0073] According to the embodiment, step b2) may be performed before step b3), or step b3) may be performed before step b2), or steps b2) and b3) may be performed concomitantly.
[0074] Furthermore, according to an embodiment, the order may be as follows: b1), b3), b4) and b2).
[0075] The conditions of temperature, pressure and contact time detailed above for step b) apply to steps b2) and b3) as described above.
[0076] Preferably, step b2) is carried out at a pressure of at least 74 bar (7.4 MPa).
[0077] Preferably, step b3) is carried out at a temperature of at least 30°C.
[0078] The flow rate of introducing the supercritical fluid into the container in step b4) is not particularly limited. A person skilled in the art can determine the flow rate based on the device used and the amount and concentration of the LiFSi solution.
[0079] Step b4) can be carried out batchwise, continuously or semi-continuously.
[0080] Preferably, the supercritical fluid used in step b) comprises supercritical carbon dioxide (sCO2). sCO2 is a fluid state of carbon dioxide maintained at or above its critical temperature (31.0°C) and critical pressure (7.3773MPa).
[0081] Advantageously, the supercritical fluid used in step b) consists essentially of sCO2, or it comprises sCO2.
[0082] According to an embodiment, sCO2 is mixed with up to 10 wt.% ethanol, for example with 0.1 to 8 wt.% ethanol, the wt.% being based on the total weight of the supercritical fluid and the ethanol.
[0083] The process of the present invention can be carried out in batch mode, in continuous or semi-continuous mode.
[0084] According to an embodiment, the method is carried out in a continuous or semi-continuous manner.
[0085] For example, according to the present invention, the injection of the LiFSI solution into the container can be performed in a continuous or semi-continuous manner. In other words, according to an embodiment, the LiFSI solution is continuously injected into the container, or alternatively, the LiFSI solution is semi-continuously injected into the container. For example, the LiFSI solution can be injected into the container for a certain time (e.g., between 30 seconds and 120 seconds, such as 60 seconds), and then the injection is stopped for another period of time, which period of time can be equal to, shorter than, or longer than the injection time.
[0086] For example, according to the present invention, the supercritical fluid may be introduced into the vessel in a continuous or semi-continuous manner.
[0087] For example, the method of the present invention may include the step of continuously or semi-continuously withdrawing the LiFSI salt from the container.
[0088] The LiFSI in solid form recovered in step c) is preferably in the form of a powder.
[0089] In step c), once step b) is completed or while step b) is ongoing, LiFSi in solid form may be recovered.
[0090] According to a specific embodiment of step c), solid LiFSI flows into a separator together with a supercritical fluid. The pressure is released and the supercritical fluid becomes a gas. This gas is preferably recycled, as described in detail below.
[0091] The method of the present invention may further comprise additional steps, for example at least one step comprising recycling the solvent and / or recycling the supercritical fluid.
[0092] Advantageously, the process of the invention comprises recycling of the solvent and recycling of the supercritical fluid.
[0093] For example, the supercritical fluid may be reinjected into the process of the invention as such or after an additional purification step or steps.
[0094] For example, the recycled solvent can be reused in a different process, such as an upstream process for preparing LiFSI salt.
[0095] Recycling of the solvent and / or supercritical fluid can be performed in several ways.
[0096] According to an embodiment, the supercritical fluid may be recirculated in a continuous manner during the method. Preferably, it is recirculated under pressure using a supercritical fluid tube.
[0097] According to another embodiment, the supercritical fluid may be recovered as a liquid phase by releasing the pressure in the container and then repressurizing it in its gaseous form, for example with the aid of a compressor, in order to recirculate it as a supercritical fluid that can be discharged in the container.
[0098] The method of the present invention can be carried out in an apparatus comprising:
[0099] a container which withstands the pressures and temperatures used, for example a pressure P of at least 73 bar and a temperature P above 30° C.;
[0100] -Solvent trap;
[0101] - Gas tanks and supercritical gas generators;
[0102] -optionally, a solution tank;
[0103] - at least one syringe / inlet valve mounted on the container; and
[0104] -Optionally, a separator.
[0105] The container may preferably be made of sapphire, SS316L, glass or graphite filled PTFE.
[0106] The container may notably be a column or an autoclave.
[0107] The device may include a separator. Different separators may be used in the method of the present invention. In some embodiments, the separation of liquid and gas / fluid may be performed by conventional filtration (also referred to as "dead-end filtration") or cross filtration (also referred to as tangential filtration), as disclosed, for example, in US2007 / 0021570 (in the name of Solvay SA). Alternatively, a cyclone separator may be used, such as those operated as a liquid / solid or gas / solid separator. A cyclone separator is advantageous because it allows the recovery of solids that may clog the filter medium. There are several mixing devices based on this principle. It is noteworthy that reference may be made to patent US 7,410,620 (in the name of North Carolina State University).
[0108] Preferably, solid LiFSI is recovered via a frit filter at the end of the process.
[0109] For example, the glass frit filter may be made of stainless steel. Preferably, the glass frit filter has at least one of the following features:
[0110] - a pore size between 1 and 6 μm, preferably 2 to 4 μm;
[0111] - a diameter between 1 and 20 mm, preferably between 5 and 15 mm, more preferably about 10 mm; and / or
[0112] - a thickness of 0.1 to 5 mm, preferably between 0.7 and 3.5 mm, more preferably between 1.5 and 2.5 mm.
[0113] If the device comprises a filter or several filters, the filter or filters may notably be placed at the bottom or at the top of the container.
[0114] A second object of the present invention relates to the lithium salt of bis(fluorosulfonyl)imide (LiFSI) in solid form obtainable by the process of the present invention.
[0115] Advantageously, such a LiFSI salt is characterized by containing solvent in an amount less than 50 ppm as measured by Li NMR.
[0116] The amount of solvent in LiFSI in solid form (eg, in powder form) is preferably less than 40 ppm, less than 30 ppm, less than 20 ppm, less than 10 ppm, or even less than 5 ppm.
[0117] The LiFSI salt of the present invention also preferably exhibits at least one of the following chemical entity contents (as measured by ion chromatography):
[0118] - less than 10,000 ppm, preferably less than 5,000 ppm, more preferably less than 1,000 ppm, more preferably less than 500 ppm, more preferably less than 100 ppm, more preferably less than 50 ppm, more preferably less than 20 ppm of fluoride ion (F - ) content; and / or
[0119] - less than 30,000 ppm, preferably less than 10,000 ppm, more preferably less than 5,000 ppm, even more preferably less than 1,000 ppm, still more preferably less than 100 ppm, more preferably less than 50 ppm and still more preferably less than 20 ppm of sulfate (SO4 2- ) content; and / or
[0120] - less than 10,000 ppm, preferably less than 5,000 ppm, more preferably less than 1,000 ppm, more preferably less than 500 ppm, more preferably less than 100 ppm, more preferably less than 50 ppm, more preferably less than 20 ppm, more preferably less than 8 ppm of chloride ions (Cl - ) content; and / or
[0121] - an iron (Fe) content of less than 1,000 ppm, preferably less than 800 ppm, more preferably less than 500 ppm; and / or
[0122] - a chromium (Cr) content of less than 1,000 ppm, preferably less than 800 ppm, more preferably less than 500 ppm; and / or
[0123] - a nickel (Ni) content of less than 1,000 ppm, preferably less than 800 ppm, more preferably less than 500 ppm; and / or
[0124] - a zinc (Zn) content of less than 1,000 ppm, preferably less than 100 ppm, more preferably less than 10 ppm, and / or
[0125] - a copper (Cu) content of less than 1,000 ppm, preferably less than 100 ppm, more preferably less than 10 ppm; and / or
[0126] - a bismuth (Bi) content of less than 1,000 ppm, preferably less than 100 ppm, more preferably less than 10 ppm; and / or
[0127] - a sodium (Na+) content of less than 10,000 ppm, preferably less than 5 000 ppm, more preferably less than 500 ppm; and / or
[0128] - less than 10,000 ppm, preferably less than 5 000 ppm, more preferably less than 500 ppm potassium (K+ )content.
[0129] According to a third object, the present invention relates to a powder comprising a lithium salt of bis(fluorosulfonyl)imide (LiFSI) and at least one other substance selected from:
[0130] - a solvent, preferably in an amount of less than 50 ppm as measured by Li NMR; and / or
[0131] - water, preferably in an amount of up to or less than 50 ppm as measured by KF; and / or
[0132] -Fluoride ion (F - ), preferably in an amount less than 25 ppm; and / or
[0133] -Chloride ion (Cl - ), preferably in an amount less than 8 ppm; and / or
[0134] -Sulfate (SO4 2- ), preferably in an amount less than 20 ppm; and / or
[0135] - Acidic substances, preferably in an amount less than 1 ppm.
[0136] Preferably, the solvent mentioned herein above is the same solvent used in the LiFSI solution, as provided in step (a).
[0137] Preferably, the acidic substance is selected from NH2SO3 - and / or FSO3 - .
[0138] Advantageously, said powder as defined above is obtainable by the process according to the invention.
[0139] A fourth object of the present invention relates to the use of the lithium salt of bis(fluorosulfonyl)imide (LiFSI) of the present invention in a battery electrolyte solution.
[0140] A fifth object of the present invention relates to the use of supercritical fluid extraction for the preparation of LiFSI in solid form from a solution comprising a lithium salt of bis(fluorosulfonyl)imide (LiFSI) and at least one solvent.
[0141] Should the disclosure of any patents, patent applications, and publications incorporated herein by reference conflict with the description of the present application to the extent that it renders a term unclear, the present description shall take precedence.
[0142] The present invention will now be described in more detail with reference to the following examples, which are for illustrative purposes only and are not intended to limit the scope of the present disclosure.
[0143] Examples
[0144] Example 1 - Preparation of LiFSI solution
[0145] LiFSI solution is prepared as follows. The method is carried out in a 1L reactor with a stirring device, a double jacket for heat regulation, a condenser, a pressure regulator device and a liquid or gas addition device under N2. At room temperature, 577.18g of ethyl methyl carbonate (EMC) is introduced, and 145.77g of anhydrous NH4F is suspended. 190.52g of bis(chlorosulfonyl)imide (HCSI) with the formula (Cl-SO2)2-NH is gradually added during 1 hour, and the mixture is heated to less than 75 ° during 18-20 hours under stirring. The mixture is cooled to room temperature, and 0.945g of 25% NH4OH (aqueous solution) (ammonia) is added. The obtained mixture is stirred at room temperature for 2 hours and then filtered.
[0146] Then product is concentrated to 866.18g, and 247.5g concentrated solution is transferred in glass reactor.In 1 hour, slowly add 371.3g methylene chloride.Precipitated NH4FSI is filtered, washed with methylene chloride, and dried in vacuum drying oven, to obtain 144.5g NH4FSI as white solid.
[0147] 110.12 g of crystalline NH4FSI was dissolved in 902.7 g of EMC. 23.37 g of a 25 wt.% aqueous solution of LiOH.H2O was added. The resulting biphasic mixture was stirred at room temperature for 1 hour and then decanted. The organic phase was recovered and precipitated under reduced pressure (10 -1 bar) and placed in a thin film evaporator at 60°C.
[0148] A solution of 30 wt.% LiFSI in EMC was obtained.
[0149] Example 2 - Preparation of LiFSI in powder form starting from the LiFSI solution of Example 1
[0150] use Figure 1 The equipment was set up and the experiment was performed as follows.
[0151] 8.907 g of LiFSI solution (2.67 g of LiFSI) obtained following the procedure in Example 1 was introduced into the container. The container was pressurized with sCO2 (temperature 45°C; pressure 200 bar). The outlet valve was then opened to the desired level to set the flow rate of CO2. After a contact time of about 90 min in the container (sCO2 / LiFSI solution ratio of 3 to 80), the inlet valve between the buffer tank and the container was closed to depressurize the container and the outlet line.
[0152] result:
[0153] 2.27 g of LiFSI salt (white and dry) were isolated in the extractor. The yield of the extraction was therefore about 85%.
[0154] The water content was measured according to Karl-Fischer analysis (oven method) as follows. The samples were prepared by a fully automatic oven sample processor (Metrohm); sample weight 0.1 g, carrier gas = N2, oven temperature = 160°C. The titration was performed using a mixture of methanol and NH4F (1:1 v / v). The polarization current for the potentiometric determination of the reaction endpoint was 10 μA, and the titration endpoint voltage was 50 mV.
[0155] The water content in the sample of the LiFSI solid product was less than 50 ppm.
[0156] No major impurities were detected by ion chromatography (DIONEX ICS-3000):
[0157] -F-<20ppm
[0158] -Cl - <5ppm
[0159] -SO4 2- <15ppm
[0160] -NH2SO 3- n / d(not detected)
[0161] -FSO3 - n / d(not detected)
[0162] The purity was greater than 99.9% as determined by Li-NMR.
Claims
1. A method for preparing a lithium salt of bis(fluorosulfonyl)imide (LiFSI) in solid form, the method comprising: The following steps are involved: a) providing a solution comprising LiFSI and at least one solvent [LiFSI solution]; b) contacting the LiFSI solution with at least one supercritical fluid; and c) recovering LiFSI in solid form.
2. The method according to claim 1, in, The at least one supercritical fluid in step b) is selected from: one fluid in a supercritical state, or a mixture of at least two fluids in a supercritical state.
3. The method according to any one of claims 1 or 2, in, The LiFSI solution comprises a solvent selected from the group consisting of ethylene carbonate, propylene carbonate, butylene carbonate, γ-butyrolactone, γ-valerolactone, dimethoxymethane, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxane, 4-methyl-1,3-dioxolane, methyl formate, methyl acetate, methyl propionate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, sulfolane, 3-methylsulfolane, dimethyl sulfoxide, N,N-dimethylformamide, N-methyloxazolidinone, acetonitrile, valeronitrile, benzonitrile, ethyl acetate, isopropyl acetate, n-butyl acetate, nitromethane, nitrobenzene, trifluoroethanol, and mixtures thereof.
4. The method according to any one of claims 1 to 3, in, The LiFSI solution includes between 5 and 70 wt. % LiFSI based on the total weight of the LiFSI solution.
5. The method according to any one of claims 1 to 4, in, The LiFSI in solid form is in the form of powder.
6. The method according to any one of claims 1 to 5, in, Step b) is carried out in a vessel at a pressure P of at least 73 bar (7.3 MPa) and / or at a temperature T between 30°C and 90°C.
7. The method according to any one of the preceding claims, in, The supercritical fluid comprises CO 2 , optionally mixed with at least one polar solvent having a solubility in the supercritical fluid of less than 10 wt. %, based on the total weight of the supercritical fluid and the at least one polar solvent.
8. The method according to claim 7, in: - the pressure P in the container is comprised between 80 and 500 bar; and / or - The temperature in the container is comprised between 35°C and 80°C.
9. The method according to any one of claims 1 to 8, in, The process is carried out continuously or semi-continuously.
10. The method according to any one of claims 1 to 9, further comprising at least one step of recycling the solvent and / or recycling the supercritical fluid.
11. The method according to any one of claims 1 to 10, which is carried out in an apparatus comprising: - a container which can withstand a pressure P of at least 80 bar and a temperature P greater than 10° C.; -Solvent trap; - Gas tanks and supercritical gas generators; -optionally, a solution tank; - at least one syringe / inlet valve mounted on the container; and -Optionally, a separator.
12. A lithium salt of bis(fluorosulfonyl)imide (LiFSI) in solid form obtainable by a process according to any one of claims 1 to 11, It is characterized in that The salt contains LiFSI and a solvent in an amount less than 50 ppm as measured by Li NMR.
13. A powder comprising a lithium salt of bis(fluorosulfonyl)imide (LiFSI) and at least one other substance selected from: - a solvent, preferably in an amount of less than 50 ppm as measured by Li NMR; and / or - water, preferably in an amount of less than 50 ppm as measured by KF; and / or -Fluoride ion (F - ), preferably in an amount of less than 25 ppm as measured by ion chromatography (IC); and / or -Chloride ion (Cl - ), preferably in an amount of less than 8 ppm as measured by IC; and / or -Sulfate (SO 4 2- ), preferably in an amount of less than 20 ppm as measured by IC; and / or - Acidic substances, preferably in an amount of less than 1 ppm as measured by IC.
14. Use of the lithium salt of bis(fluorosulfonyl)imide (LiFSI) in solid form according to claim 12 or the powder according to claim 13 in a battery electrolyte solution.
15. Use of supercritical fluid extraction for preparing a lithium salt of bis(fluorosulfonyl)imide (LiFSI) in solid form from a solution comprising LiFSI and at least one solvent.
Citation Information
Patent Citations
Polymeric ultraviolet light stabilisers containing hindered alkyl amines and polymer compositions containing them
EP0002022A1
Method for producing alkali metal salt of fluorosulfonyl imide
JP2014201453A
Manufacturing method of fluorosulfonylimide compound
JP2016145147A
System and method for removing an electrolyte from an energy storage and / or conversion device using a supercritical fluid
US20030186110A1
Process for preparing a halogenated polymer and device for its implementation
US20070021570A1