Finishing agent for aftertreatment of glass fiber filter material
A finishing agent and filter material technology, which is applied in the field of glass fiber filter material post-processing technology, can solve the problems of reduced service life, poor flexibility and folding resistance of glass fiber filter material, and achieves uniform distribution, water and oil repellency. Good and water-saving effect
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2013-05-01
Smart Images
Figure 1 Figure 2 Figure 3
Abstract
Description
technical field
[0001] The invention relates to a post-treatment process of glass fiber filter material in the field of high-temperature flue gas dust removal, specifically a finishing agent for post-treatment of glass fiber filter material. Background technique
[0002] The smoke and dust produced by the iron and steel industry, metallurgical industry and cement industry not only have high temperature and high concentration, but also have very complex components, which seriously pollute the air environment. With the rapid development of the economy and the continuous enhancement of people's awareness of environmental protection, the country has paid more and more attention to environmental protection issues. Especially in the field of heavy smoke pollution, strict industry emission standards have been formulated. The emission requirements of smoke particles in many industries are lower than 50mg / m 3 .
[0003] Glass fiber is more and more favored by the environmental prote...
Examples
Embodiment 1
[0028] (1) Production of filter material: use glass fiber with a fineness of 5.5 μm and a length of 51 mm to prepare the filter material. The two layers are non-woven layers, and the middle layer is made of woven fabric. The weight is 708 g / m 2 , thickness 2.0mm.
[0029] (2) Preparation of finishing agent: polytetrafluoroethylene dispersion emulsion 350ml / L, high temperature resistant fluorine-containing polyacrylate softener 455ml / L, silicone water repellent agent 85ml / L, siloxane coupling agent 4.2ml / L L. Emulsifier 0.6ml / L, Catalyst 0.10g / L, Anionic Foaming Agent 3.0g / L, Penetrant 2.8g / L, Stabilizer 12.2g / L, Stir each raw material in the formula and add water Make up to 1 liter, and make the finishing solution uniform through mechanical stirring, and the viscosity of the finishing solution is 68mPa s.
[0030] Wherein, the solid content of the polytetrafluoroethylene dispersion emulsion is 40%, and the pH value is 7; the emulsifier is triethanolamine fatty acid salt; the ...
Embodiment 2
[0038] (1) Production of filter material: use glass fiber with a fineness of 4.5 μm and a length of 60 mm to prepare the filter material. The two layers are non-woven layers, and the middle layer is made of woven fabric. The weight is 685 g / m 2 , thickness 1.9mm.
[0039] (2) Preparation of finishing agent: PTFE dispersion emulsion 400ml / L, high temperature resistant fluorine-containing polyacrylate softener 400ml / L, silicone water repellent agent 110ml / L, siloxane coupling agent 4.7ml / L L. Emulsifier 0.69ml / L, catalyst 0.22g / L, anionic foaming agent 9.8g / L, penetrant 16.6g / L, stabilizer 18.5g / L, mix the raw materials in the formula evenly and add water Make up to 1 liter, and make the finishing solution uniform through mechanical stirring, and the viscosity of the finishing solution is 82mPa s.
[0040] Wherein, the polytetrafluoroethylene dispersed emulsion has a solid content of 75% and a pH value of 8; the emulsifier is polyoxyethylene alkylphenol ether sulfate; the inorg...
Embodiment 3
[0047] (1) Production of filter material: use glass fiber with a fineness of 5.5 μm and a length of 51 mm to prepare the filter material. The two layers are non-woven layers, and the middle layer is made of woven fabric. The weight is 740 g / m 2 , thickness 1.8mm.
[0048] (2) Preparation of finishing agent: polytetrafluoroethylene dispersion emulsion 620ml / L, high temperature resistant fluorine-containing polyacrylate softener 100ml / L, silicone water repellent agent 170ml / L, siloxane coupling agent 8.7ml / L L. Emulsifier 1.92ml / L, inorganic salt catalyst 1.55g / L, anionic foaming agent 20g / L, penetrant 38g / L, stabilizer 20g / L, mix all raw materials in the formula and add water Make up to 1 liter, and make the finishing solution uniform by mechanical stirring, and the viscosity of the finishing solution is 82mPa·s.
[0049] Among them, the solid content of the polytetrafluoroethylene dispersion emulsion is 55%, and the pH value is 7.5; the emulsifier is an alkyl sulfonate; the c...