Adhesive film and dicing die bonding integrated film

By adjusting the resin composition and filler mixing amount in the adhesive film, the problem that the adhesive film in the prior art is difficult to take into account high thermal conductivity and adhesive strength, and the balance between efficient heat dissipation and bonding performance is achieved.

CN109155244BActive Publication Date: 2024-11-26RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201780024601.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2016-06-10
Filing Date
2017-06-09
Publication Date
2024-11-26
Estimated Expiration
2037-06-09

AI Technical Summary

Technical Problem

In the prior art, when the adhesive film of a semiconductor element improves heat dissipation, it is difficult to take into account both high adhesion and heat dissipation, and excessive increase of fillers may lead to insufficient adhesive strength.

Method used

Adhesive films containing polymers, liquid epoxy resins, curing agents and curing accelerators at 50°C, and the amount of ring structures and filler mixing in the resin component are adjusted to ensure that the thermally cured adhesive film has High thermal conductivity and sufficient adhesive force.

Benefits of technology

The balance between high thermal conductivity and high adhesive force is achieved, ensuring effective heat dissipation and bonding performance of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109155244B_ABST
    Figure CN109155244B_ABST
Patent Text Reader

Abstract

The present disclosure relates to an adhesive film having thermosetting properties. The adhesive film contains: (a) a polymer; (b) an epoxy resin that is liquid at 50°C; (c) at least one of a curing agent and a curing accelerator; and (d) a filler having a thermal conductivity of 10 W / (m·K) or more, and satisfies the conditions shown in the following inequality (1), and the shear strength after thermosetting is 1.5 MPa or more. In the formula, ma represents the carbon mass that forms the cyclic structure of (a) the polymer, mb represents the carbon mass that forms the cyclic structure of (b) the epoxy resin, mc represents the carbon mass that forms the cyclic structure of (c) the curing agent and the curing accelerator, and M represents the total mass of (a) the polymer, (b) the epoxy resin, and (c) the curing agent and the curing accelerator. (ma+mb+mc) / M≥0.43 (1).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an adhesive film and a dicing die bonding integrated film. Background Art

[0002] In the past, various technologies for improving the heat dissipation effect of semiconductor devices have been proposed. Patent document 1 discloses a semiconductor device package that improves the heat dissipation effect of heat generated by semiconductor elements by providing a metal base under a dicing pad and a lead portion on which semiconductor elements are placed. Patent document 2 discloses that particles having a thermal conductivity of 12 W / (m·K) or more are incorporated into a thermosetting die bonding film, thereby increasing the thermal conductivity of the die bonding film after thermal curing to 1 W / (m·K) or more.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 5-198701

[0006] Patent Document 2: Japanese Patent Application Publication No. 2015-103573 Summary of the invention

[0007] Technical problem to be solved by the invention

[0008] However, the invention described in Patent Document 1 still has room for improvement in the following aspects: That is, since the metal substrate used in the invention described in Patent Document 1 has a different thermal expansion coefficient from the semiconductor element and the dicing pad, there is a risk that the metal substrate may peel off or cracks may occur in the semiconductor package due to repeated heating of the semiconductor element.

[0009] Although Patent Document 2 discloses a film having a thermal conductivity of 1 W / (m·K) or more after thermal curing, further high thermal conductivity of the film is expected. The thermal conductivity of the adhesive film can be further improved by further increasing the amount of filler with high thermal conductivity. However, when the amount of filler is excessively increased, the amount of resin is relatively reduced. As a result, the adhesive force (shear strength after curing) of the adhesive film tends to become insufficient, and it becomes difficult to play the role of the adhesive that it should have. That is, it is difficult to take into account both excellent adhesion and heat dissipation by simply adjusting the amount of filler with high thermal conductivity.

[0010] The present disclosure has been made in view of the above-mentioned problems, and an object of the present disclosure is to provide an adhesive film capable of achieving both adhesiveness and heat dissipation at sufficiently high levels, and a dicing die bonding integrated film including the adhesive film as a die bonding film.

[0011] Means for solving technical problems

[0012] The present disclosure relates to a thermosetting adhesive film, which contains: (a) a polymer; (b) an epoxy resin that is liquid at 50°C; (c) at least one of a curing agent and a curing accelerator; and (d) a filler having a thermal conductivity of 10 W / (m·K) or more. The adhesive film satisfies the conditions shown in the following inequality (1), and has a shear strength of 1.5 MPa or more after thermosetting.

[0013] (ma+mb+mc) / M≥0.43 (1)

[0014] [In the formula, ma represents the mass of carbon forming the cyclic structure of (a) the polymer, mb represents the mass of carbon forming the cyclic structure of (b) the epoxy resin, mc represents the mass of carbon forming the cyclic structure of (c) the curing agent and the curing accelerator, and M represents the total mass of (a) the polymer, (b) the epoxy resin, and (c) the curing agent and the curing accelerator.]

[0015] The present disclosure can adopt the following configurations.

[0016] The arithmetic mean roughness Ra of the film surface after thermal curing is 0.25 μm or less.

[0017] (a) The polymer includes a polymer satisfying the condition represented by the following inequality (2).

[0018] ma / M A ≥0.40 (2)

[0019] [wherein, ma represents the carbon mass of the cyclic structure forming the polymer (a), M A represents (a) the total mass of the polymer.]

[0020] (a) The polymer contains a phenoxy resin.

[0021] (d) The filler is α-alumina particles.

[0022] The thickness of the adhesive film is 50 μm or less.

[0023] The content of the filler (d) is 60 to 95 parts by mass when the total amount of the (a) polymer, (b) epoxy resin, (c) curing agent and curing accelerator, and (d) filler is 100 parts by mass.

[0024] The present disclosure provides a dicing die bonding integrated film including the above-mentioned adhesive film as a die bonding film. That is, the dicing die bonding integrated film includes: a die bonding film formed of the above-mentioned adhesive film; and a dicing film laminated on the die bonding film.

[0025] Effects of the Invention

[0026] According to the present disclosure, it is possible to provide an adhesive film capable of achieving both adhesiveness and heat dissipation at sufficiently high levels, and a dicing die bonding integrated film including the adhesive film as a die bonding film. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a cross-sectional view schematically showing one embodiment of the dicing die bonding integrated film disclosed in the present invention. DETAILED DESCRIPTION

[0028] The following is a detailed description of the embodiments of the present disclosure. The adhesive film of the present embodiment is thermosetting and contains a resin component formed by (a) a polymer, (b) an epoxy resin that is liquid at 50°C, (c) a curing agent and a curing accelerator, and (d) a filler (with a thermal conductivity of 10 W / (m·K) or more) dispersed in the resin component. The adhesive film is completed based on the new insight that the thermal conductivity of the cured adhesive film can be improved by increasing the amount of cyclic structures (especially aromatic rings) in the above-mentioned resin component. That is, the adhesive film of the present embodiment achieves an improvement in the thermal conductivity of the cured adhesive film by replacing the existing method of adjusting the amount of fillers with high thermal conductivity, or by adjusting the amount of cyclic structures in the resin component in addition to the existing method.

[0029] The adhesive film of the present embodiment satisfies the condition represented by the following inequality (1), and has a shear strength of 1.5 MPa or more after thermal curing.

[0030] (ma+mb+mc) / M≥0.43 (1)

[0031] [In the formula, ma represents the mass of carbon forming the ring structure of (a) the polymer, mb represents the mass of carbon forming the ring structure of (b) the epoxy resin, mc represents the mass of carbon forming the ring structure of (c) the curing agent and curing accelerator, and M represents the total mass of (a) the polymer, (b) the epoxy resin, and (c) the curing agent and curing accelerator.]

[0032] The amount of aromatic rings of the components (polymer, epoxy resin, and curing agent and / or curing accelerator) constituting the resin component can be evaluated using the ring parameter. The larger the value of the ring parameter, the greater the amount of aromatic rings. The ring parameter is a value calculated by dividing the carbon mass of the aromatic rings forming the compound by the total mass of the compound. When preparing the resin component, as a polymer, epoxy resin, curing agent or curing accelerator, by selecting a substance with a large value of the ring parameter, the value on the left side of the above inequality (1) can be increased.

[0033] By using a resin component that satisfies the conditions shown in inequality (1), an adhesive film having sufficiently high thermal conductivity after curing can be obtained even if the amount of filler (d) is excessively increased. From the viewpoint of obtaining an adhesive film having higher thermal conductivity after curing, the resin component preferably satisfies the following inequality (1A), and more preferably satisfies the following inequality (1B).

[0034] (ma+mb+mc) / M≥0.45 (1A)

[0035] (ma+mb+mc) / M≥0.47 (1B)

[0036] The upper limit value of ((ma+mb+mc) / M) is, for example, approximately 0.70. If the upper limit value is exceeded, the film becomes hard and the adhesiveness tends to be insufficient.

[0037] The thermal conductivity of the adhesive film after thermal curing is preferably 1.3 W / (m·K) or more, more preferably 1.5 W / (m·K) or more, and further preferably 1.7 W / (m·K) or more. When the thermal conductivity of the adhesive film after curing is 1.3 W / (m·K) or more, when the adhesive film is used as a chip bonding film to manufacture a semiconductor device, a sufficient heat dissipation effect can be obtained. The upper limit of the thermal conductivity of the adhesive film after curing is, for example, 6.0 W / (m·K) and can also be 4.0 W / (m·K).

[0038] The shear strength of the adhesive film after thermal curing is 1.5 MPa or more, preferably 1.6 MPa or more, and more preferably 1.7 MPa or more. When the shear strength of the adhesive film after curing is 1.5 MPa or more, a sufficiently high adhesive force can be ensured. The upper limit of the shear strength of the adhesive film after curing is, for example, 10.0 MPa.

[0039] The arithmetic mean roughness Ra (hereinafter simply referred to as "surface roughness Ra") of the adhesive film after thermal curing is preferably 0.25 μm or less, more preferably 0.20 μm or less, and further preferably 0.16 μm or less. The surface roughness Ra of the adhesive film after curing is 0.25 μm or less, which can ensure a sufficiently high adhesive force. The lower limit of the surface roughness Ra of the adhesive film after curing is, for example, 0.03 μm.

[0040] The thickness of the adhesive film may be 50 μm or less, for example, 5 to 50 μm, preferably 5 to 40 μm, and more preferably 8 to 40 μm. When the thickness of the adhesive film is less than 5 μm, the stress relaxation effect tends to be insufficient and the embedding property tends to be reduced, while when the thickness exceeds 50 μm, the cost tends to be high.

[0041] The components contained in the adhesive film are described below.

[0042] <(a) Polymer>

[0043] As (a) polymer, from the viewpoint of obtaining film formation, heat resistance and adhesion, preferably phenoxy resin, polyimide resin, polyamide resin, polycarbodiimide resin, cyanate resin, acrylic resin, polyester resin, polyethylene resin, polyethersulfone resin, polyetherimide resin, polyvinyl acetal resin and polyurethane resin. Among them, from the viewpoint of excellent film formation and heat resistance, more preferably phenoxy resin, polyimide resin, polyamide resin, acrylic resin, cyanate resin and polycarbodiimide resin, from the viewpoint of easy adjustment such as molecular weight and characteristic imparting, more preferably phenoxy resin. As (a) polymer, one selected from the above-mentioned resin can be used alone, or two or more can be used in combination, and copolymers of two or more monomers can also be used.

[0044] From the viewpoint of increasing the left-hand side value ((ma+mb+mc) / M) of the above inequality (1), the (a) polymer preferably contains a polymer satisfying the conditions shown in the following inequality (2), more preferably satisfying the following inequality (2A), and even more preferably satisfying the following inequality (2B).

[0045] ma / M A ≥0.40 (2)

[0046] ma / M A ≥0.45 (2A)

[0047] ma / M A ≥0.50 (2B)

[0048] [where ma represents the carbon mass forming the cyclic structure of the polymer, M A represents the total mass of the polymer.]

[0049] In other words, the polymer (a) preferably consists of one or more polymers, and the ring parameter of at least one of the polymers is preferably 0.40 or more, more preferably 0.45 or more, and even more preferably 0.50 or more.

[0050] When a phenoxy resin is used as the polymer (a), the weight average molecular weight thereof is preferably 20,000 or more, more preferably 30,000 or more. Examples of commercially available phenoxy resins include YP-50, YP-55, YP-70, YPB-40PXM40, YPS-007A30, FX-280S, FX-281S, FX-293, and ZX-1356-2 (all manufactured by Tohto Kasei Co., Ltd., trade names), 1256, 4250, 4256, 4275, YX7180, YX6954, YX8100, YX7200, YL7178, YL7290, YL7600, YL7734, YL7827, and YL7864 (all manufactured by Japan Epoxy Resin Co., Ltd., trade names), and the like. One of these may be used alone or two or more of these may be used in combination.

[0051] The glass transition temperature (Tg) of the phenoxy resin is preferably lower than 85° C., and commercial products satisfying this condition include, for example, YP-50, YP-55, YP-70, ZX-1356-2 (all manufactured by Tohto Kasei Co., Ltd., trade names); 4250, 4256, 7275, YX7180, and YL7178 (all manufactured by Japan Epoxy Resin Co., Ltd., trade names). One of these may be used alone, or two or more may be used in combination.

[0052] When an acrylic resin is used as the (a) polymer, it is preferably one having a reactive group (functional group) and a weight average molecular weight of 100,000 or more. As the reactive group, for example, carboxylic acid group, amino group, hydroxyl group and epoxy group can be cited. Among them, when the functional group monomer is a carboxylic acid type acrylic acid, there is a situation where the adhesion decreases due to the ease of cross-linking reaction, gelation in the varnish state, and the increase in the degree of curing in the B stage state. Therefore, it is more preferred to use glycidyl acrylate or glycidyl methacrylate with an epoxy group that does not occur or even if it occurs, the period is very long. Among acrylic resins, it is more preferred to use an acrylic copolymer containing an epoxy group with a weight average molecular weight of 100,000 or more. (a) The polymer can be obtained by polymerizing in a manner that unreacted monomers remain in the polymerization reaction to obtain the polymer compound, or it can also be obtained by adding a monomer containing a reactive group after obtaining the polymer compound. In addition, the weight average molecular weight is a polystyrene conversion value obtained by gel permeation chromatography (GPC) using a standard curve obtained from standard polystyrene.

[0053] As an acrylic copolymer, for example, an acrylic rubber which is a copolymer of acrylate, methacrylate, and acrylonitrile can be cited. In addition, due to high adhesiveness and heat resistance, an acrylic copolymer containing 0.5 to 6% by mass of glycidyl acrylate or glycidyl methacrylate as a functional group, having a glass transition temperature (Tg) of -50°C or more and 50°C or less, further -10°C or more and 50°C or less, and having a weight average molecular weight of 100,000 or more is particularly preferred. As an acrylic copolymer containing 0.5 to 6% by mass of glycidyl acrylate or glycidyl methacrylate, having a Tg of -10°C or more and a weight average molecular weight of 100,000 or more, for example, HTR-860P-3 (manufactured by Imperial Chemical Industry Co., Ltd., trade name) can be cited.

[0054] The amount of glycidyl acrylate or glycidyl methacrylate used as a functional group monomer is preferably 2 to 6% by mass of the copolymer ratio. In order to obtain a higher adhesive force, it is preferably 2% or more by mass. When it exceeds 6% by mass, gelation may occur. The remainder can be a mixture of alkyl acrylates, alkyl methacrylates, styrene, acrylonitrile, etc. having an alkyl group with a carbon number of 1 to 8, such as methyl acrylate and methyl methacrylate. Among them, ethyl (meth)acrylate and / or butyl (meth)acrylate are particularly preferred. From the viewpoint of increasing the value on the left side of the above inequality (1) ((ma+mb+mc) / M), styrene, benzyl acrylate or benzyl methacrylate is preferably used as a functional group monomer. The mixing ratio is preferably adjusted in consideration of the Tg of the copolymer. When Tg is less than -10°C, there is a tendency for the adhesion of the adhesive layer or adhesive film in the B stage state to increase, and sometimes the handling property will deteriorate. The polymerization method is not particularly limited, and examples thereof include bead polymerization, solution polymerization, etc., by which the copolymer is obtained.

[0055] The weight average molecular weight of the epoxy-containing acrylic copolymer is preferably 300,000 to 3,000,000, and more preferably 400,000 to 2,000,000. When the weight average molecular weight is less than 300,000, the strength or flexibility of the adhesive film (or adhesive sheet) may be reduced, or the adhesion may be increased, while when it exceeds 3,000,000, the fluidity may be reduced, and the circuit filling property of the wiring may be reduced.

[0056] The content of the polymer (a) in the adhesive film is preferably 3 to 40 parts by mass, more preferably 3 to 30 parts by mass, and even more preferably 3 to 20 parts by mass, relative to 100 parts by mass of the total amount of the polymer (a), the epoxy resin (b), the curing agent and the curing accelerator (c), and the filler (d). When the content of the polymer (a) is 3 parts by mass or more, the elastic modulus can be appropriately reduced while providing fluidity during molding. When the content exceeds 40 parts by mass, the fluidity may be reduced when the attachment load is small, and the circuit filling property may be reduced.

[0057] <(b) Epoxy resin>

[0058] As the (b) epoxy resin, an epoxy resin having difunctional groups or more and a molecular weight preferably less than 5000, more preferably less than 3000 can be used, for example, difunctional epoxy resins such as bisphenol A epoxy resin and bisphenol F epoxy resin, novolac epoxy resins such as phenol novolac epoxy resin and cresol novolac epoxy resin, etc. In addition, commonly known epoxy resins such as multifunctional epoxy resins and heterocyclic epoxy resins can also be used.

[0059] Examples of commercially available epoxy resins include Epikote 152, Epikote 154, Epikote 604, Epikote 630, Epikote 630LSD, Epikote 807, Epikote 815, Epikote 825, Epikote827, Epikote 828, Epikote 834, and Epikote 1001, Epikote 1002, Epikote 1003, Epikote 1055, Epikote 1004, Epikote 1004AF, Epikote 1007, Epikote 1009, Epikote 1003F, Epikote1004F, Epikote 180S65, Epon 1031S, Epikote 1032H60, Epikote 157S70, 1256, 4250, 4256, 4275, YX6954, YX8100, YL7178, YL7290, YL7175-500, YL7175-1000 (all manufactured by Japan Epoxy Resin Co., Ltd., trade names), DER-330, DER-301, DER-361, DER-661, DER-662, DER-663U, DER-664, DER-664U, DER-667, DER-642U, DER-672U, DER-673MF, DER-668, DER-669, DEN-438 (all manufactured by Dow Cresol novolac epoxy resins such as YDCN-700, YDCN-701, YDCN-702, YDCN-703, YDCN-704, YD-8125, YDF-8170, YDF-8170C, YD-825, YDF-870, YDF-2004, YH-434 (all manufactured by Tohto Chemical Co., Ltd., trade names), ESCN-195X, ESCN-200L, ESCN-220 Amine type epoxy resins such as esters, ELM-120 (all manufactured by Sumitomo Chemical Co., Ltd.), EPPN-201, EPPN501H, EPPN502H, RE-3035-L, RE-310S, EOCN-102S, EOCN-103S, EOCN-104S, EOCN-1012, EOCN-1020, EOCN-1025, EOCN-1027 (all manufactured by Nippon Kayaku Co., Ltd.), Araldit ECN1273, AralditECN1280, Araldit ECN1299, Araldit 0163, AralditPT810 (all manufactured by Ciba Specialty Chemicals, trade names), Denacol EX-611, Denacol EX-614, Denacol EX-614B, Denacol EX-622, Denacol EX-512, Denacol EX-521, Denacol EX-421, Denacol Alicyclic epoxy resins such as EX-411, Denacol EX-321 (all manufactured by NAGASE Chemicals Co., Ltd.), TETRAD-X, TETRAD-C (all manufactured by Mitsubishi Gas Chemical Co., Ltd.), ERL4234, ERL4299, ERL4221, ERL4206 (all manufactured by UCC Corporation), EP-4000, EP-3950L, EP-3980S, EPR-4030 (all manufactured by ADEKA Co., Ltd.), etc., can be used alone or in combination of two or more.

[0060] As (b) epoxy resin, one or more types that are liquid at 50°C are used. According to the research of the present inventors, in order to manufacture an adhesive film that can take into account both adhesion and heat dissipation, it is useful to satisfy inequality (1) and maintain the flexibility of the adhesive film. For example, even if inequality (1) is satisfied, if the adhesive film is too hard, the adhesion becomes insufficient, and thus the thermal conductivity tends to become insufficient. In order to maintain the flexibility of the adhesive film, an epoxy that is liquid at 50°C is used in this embodiment. In addition, as long as the flexibility of the adhesive film can be maintained, an epoxy resin that is non-liquid at 50°C (an epoxy resin that is solid at 50°C) can also be used.

[0061] Examples of the epoxy resins that are liquid at 50° C. include Epikote 807, Epikote 815, Epikote 825, Epikote 827, Epikote 828, Epikote 834, Epikote 1001, Epikote 152, Epikote 630, and Epikote 630LSD (all of which are Japan Epoxy Resin Co., Ltd., trade name), YD-8125, YDF-8170, YD-825, YDF-870 (all manufactured by Tohto Kasei Co., Ltd., trade name), RE-3035-L, RE-310S (all manufactured by Nippon Kayaku Co., Ltd., trade name), EP-4000, EP-3950L, EP-3980S, EPR-4030 (all manufactured by Adeka Co., Ltd., trade name), etc., any one of them may be used alone, or two or more of them may be used in combination, or they may be used in combination with a solid one. From the viewpoint of increasing the value on the left side of the above inequality (1) ((ma+mb+mc) / M), it is particularly preferred that the (b) polymer contains YDF-8170 (manufactured by Tohto Kasei Co., Ltd., trade name), which also has a practical effect.

[0062] As (b) epoxy resin, when a difunctional epoxy resin and a trifunctional or higher epoxy resin are used together, when the total amount thereof is set to 100 parts by mass, the amount of the difunctional epoxy resin is preferably 50 parts by mass or more (the amount of the trifunctional or higher epoxy resin is less than 50 parts by mass). From the viewpoint of increasing Tg, it is more preferred that the amount of the difunctional epoxy resin is 50 to 90 parts by mass and the amount of the trifunctional or higher epoxy resin is 10 to 50 parts by mass.

[0063] The content of the (b) epoxy resin in the adhesive film is preferably 3 to 40 parts by mass, more preferably 3 to 30 parts by mass, and even more preferably 3 to 20 parts by mass, based on 100 parts by mass of the total amount of the (a) polymer, (b) epoxy resin, (c) curing agent and curing accelerator, and (d) filler.

[0064] <(c) Curing agent and curing accelerator>

[0065] The adhesive film of the present embodiment may contain at least one of a curing agent and a curing accelerator as the component (c). Specific examples of the curing agent and the curing accelerator are given below.

[0066] (Curing agent)

[0067] As (c) curing agent, for example, polyfunctional phenols, amines, imidazole compounds, acid anhydrides, organophosphorus compounds and their halides, polyamides, polysulfide compounds, boron trifluoride can be used. As examples of polyfunctional phenols, hydroquinone, resorcinol, catechol as monocyclic bifunctional phenols, bisphenol A, bisphenol F, bisphenol S, naphthalene diols, biphenols, and their halides, alkyl substituted products, etc. as polycyclic bifunctional phenols can be cited. In addition, phenolic resins such as phenol novolac resins, resol phenolic resins, bisphenol A novolac resins, and cresol novolac resins, which are condensation products of these phenols and aldehydes, can also be used.

[0068] Examples of commercially available preferred phenolic resin curing agents include PHENOLITE LF2882, PHENOLITE LF2822, PHENOLITE TD-2090, PHENOLITE TD-2149, PHENOLITE VH4150, and PHENOLITE VH4170 (all manufactured by Dainippon Ink & Chemicals, Ltd., trade names) and XLC series (Mitsui Chemicals, Inc., trade name).

[0069] As (c) curing agent, preferably use phenolic resin with hydroxyl equivalent of 150g / eq or more. As such phenolic resin, there is no particular limitation as long as it has the above value, but due to excellent electrical corrosion resistance during moisture absorption, preferably use phenolic varnish type or resol type resin. As a specific example of the above phenolic resin, for example, phenolic resin represented by the following formula (I) can be cited.

[0070] [Chemical formula number 1]

[0071]

[0072] [Where R 1 They may be the same or different, and represent a hydrogen atom, a linear or branched alkyl group having 1 to 10 carbon atoms, a cyclic alkyl group, an aralkyl group, an alkenyl group, a hydroxyl group, an aryl group, or a halogen atom; n represents an integer of 1 to 3, and m represents an integer of 0 to 50.]

[0073] As such a phenolic resin, there is no particular limitation as long as it conforms to formula (I). From the viewpoint of moisture resistance, it is preferred that the water absorption after being put into a constant temperature and humidity chamber at 85°C and 85%RH for 48 hours is 2% by mass or less. In addition, when a phenolic resin having a heating weight reduction rate (heating rate: 5°C / min, ambient gas: nitrogen) of less than 5% by mass at 350°C as measured by a thermogravimetric analyzer (TGA) is used, the reliability of many characteristics such as heat resistance and moisture resistance is improved because the volatile components can be suppressed during heating processing, and the machine contamination caused by the volatile components during heating processing can be reduced, so it is preferred. The phenolic resin shown in formula (I) can be obtained, for example, by reacting a phenol compound with a phenylene dimethyl compound as a divalent linking group in the absence of a catalyst or an acid catalyst.

[0074] As the phenolic resins mentioned above, for example, Mirex XLC-series and Mirex XL series (the above are trade names of Mitsui Chemicals, Inc.) can be cited. The amount of the phenolic resin when used in combination with the epoxy resin is preferably 0.70 / 0.30 to 0.30 / 0.70, more preferably 0.65 / 0.35 to 0.35 / 0.65, further preferably 0.60 / 0.30 to 0.30 / 0.60, and particularly preferably 0.55 / 0.45 to 0.45 / 0.55, in terms of the equivalent ratio of epoxy equivalent to hydroxyl equivalent. If the mixing ratio exceeds the above range, there is a possibility that the curing property will deteriorate when the adhesive is prepared.

[0075] Examples of the phenolic compound used in the production of the phenolic resin of formula (I) include phenol, o-cresol, m-cresol, p-cresol, o-ethylphenol, p-ethylphenol, o-n-propylphenol, m-n-propylphenol, p-n-propylphenol, o-isopropylphenol, m-isopropylphenol, p-isopropylphenol, o-n-butylphenol, m-n-butylphenol, p-n-butylphenol, o-isobutylphenol, m-isobutylphenol, p-isobutylphenol, octylphenol, nonylphenol, 2,4-diisobutyl ... Cresol, 2,6-xylenol, 3,5-xylenol, 2,4,6-trimethylphenol, resorcinol, catechol, hydroquinone, 4-methoxyphenol, o-phenylphenol, m-phenylphenol, p-phenylphenol, p-cyclohexylphenol, o-allylphenol, p-allylphenol, o-benzylphenol, p-benzylphenol, o-chlorophenol, p-chlorophenol, o-bromophenol, p-bromophenol, o-iodophenol, p-iodophenol, o-fluorophenol, m-fluorophenol, p-fluorophenol, etc. These phenol compounds can be used alone or in combination of two or more. Phenol, o-cresol, m-cresol, p-cresol, etc. are particularly preferred.

[0076] As the phenylenedimethyl compound as a divalent linking group used in producing the phenol resin of the formula (I), the phenylenedimethyl dihalide, phenylenedimethyl diglycol and derivatives thereof shown below can be used. That is, α,α′-dichloro-p-xylene, α,α′-dichloro-m-xylene, α,α′-dichloro-o-xylene, α,α′-dibromo-p-xylene, α,α′-dibromo-m-xylene, α,α′-dibromo-o-xylene, α,α′-diiodo-p-xylene, α,α′-diiodo-m-xylene, α,α′-diiodo-o-xylene, α,α′-dihydroxy-p-xylene, α,α′-dihydroxy-m-xylene, α,α′-dihydroxy-o-xylene, α,α′-dimethoxy-p-xylene, α,α′-dimethoxy-m-xylene, α,α′-dimethoxy-o-xylene, α,α′-diethoxy-p-xylene, α,α′-diethoxy-m-xylene, α,α′-diethyl α,α′-di-n-propoxy-p-xylene, α,α′-n-propoxy-m-xylene, α,α′-di-n-propoxy-o-xylene, α,α′-di-isopropoxy-p-xylene, α,α′-di-isopropoxy-m-xylene, α,α′-di-isopropoxy-o-xylene, α,α′-di-n-butoxy-p-xylene, α,α′-di-n-butoxy-m-xylene, α,α′-di-n-butoxy-o-xylene, α,α′-di-isobutoxy-p-xylene, α,α′-di-isobutoxy-m-xylene, α,α′-di-isobutoxy-o-xylene, α,α′-di-tert-butoxy-p-xylene, α,α′-di-tert-butoxy-m-xylene, α,α′-di-tert-butoxy-o-xylene. One of these may be used alone or two or more of them may be used in combination. Among them, preferred are α,α′-dichloro-p-xylene, α,α′-dichloro-m-xylene, α,α′-dichloro-o-xylene, α,α′-dihydroxy-p-xylene, α,α′-dihydroxy-m-xylene, α,α′-dihydroxy-o-xylene, α,α′-dimethoxy-p-xylene, α,α′-dimethoxy-m-xylene, and α,α′-dimethoxy-o-xylene.

[0077] When the phenol compound and the phenylenedimethyl compound are reacted, a mineral acid such as hydrochloric acid, sulfuric acid, phosphoric acid, polyphosphoric acid, etc.; an organic carboxylic acid such as dimethylsulfuric acid, diethylsulfuric acid, p-toluenesulfonic acid, methanesulfonic acid, ethanesulfonic acid, etc.; a superacid such as trifluoromethanesulfonic acid; a strongly acidic ion exchange resin such as an alkanesulfonic acid type ion exchange resin; a superacidic ion exchange resin such as a perfluoroalkanesulfonic acid type ion exchange resin (trade name: Nafion, manufactured by Du Pont); a natural and synthetic zeolite; an acid catalyst such as an activated clay (acid clay), etc. is used to react at 50 to 250° C. until the phenylenedimethyl compound as a raw material substantially disappears and the reaction composition becomes constant. The reaction time is approximately 1 to 15 hours, although it depends on the raw materials and the reaction temperature, and can be determined while tracking the reaction composition using GPC (gel permeation chromatography) or the like. The exception is that when a halogenated xylene derivative such as α,α′-dichloro-p-xylene is used, an acid catalyst is not required because the reaction is carried out in the absence of a catalyst while the corresponding hydrogen halide gas is generated. In other cases, the reaction is carried out in the presence of an acid catalyst to produce the corresponding water or alcohol. The reaction molar ratio of the phenol compound to the phenylene dimethyl compound is usually to use the phenol compound in excess, and the unreacted phenol compound is recovered after the reaction. At this time, the average molecular weight is determined by the amount of the phenol compound. The more excess phenol compounds are, the lower the average molecular weight of the phenolic resin can be obtained. In addition, a phenolic resin in which the phenolic compound part is allylphenol can be obtained, for example, by the following method: a phenolic resin that has not been allylated is produced, an allyl halide is reacted with it, and allyl ether is passed through, and allylation occurs by Claisen rearrangement.

[0078] Examples of amines include aliphatic or aromatic primary amines, secondary amines, tertiary amines, quaternary ammonium salts, aliphatic cyclic amines, guanidines, urea derivatives, etc. Examples of these compounds include N,N-benzyldimethylamine, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, tetramethylguanidine, triethanolamine, N,N'-dimethylpiperazine, 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]-7-undecene, 1,5-diazabicyclo[4.4.0]-5-nonene, hexamethylenetetracycline, and the like. Amine, pyridine, picoline, piperidine, pyrrolidine, dimethylcyclohexylamine, dimethylhexylamine, cyclohexylamine, diisobutylamine, di-n-butylamine, diphenylamine, N-methylaniline, tri-n-propylamine, tri-n-octylamine, tri-n-butylamine, triphenylamine, tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium iodide, triethylenetetramine, diaminodiphenylmethane, diaminodiphenyl ether, dicyandiamide, tolylbiguanide, guanyl urea, dimethyl urea, etc.

[0079] Examples of the imidazole compound include imidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-methylimidazole, 2-phenylimidazole, 2-undecylimidazole, 1-benzyl-2-methylimidazole, 2-heptadecylimidazole, 4,5-diphenylimidazole, 2-methylimidazoline, 2-phenylimidazoline, 2-undecylimidazoline, 2-heptadecylimidazole, 2-isopropylimidazole, 2,4-dimethylimidazole, 2-phenyl-4-methylimidazole, 2-ethylimidazoline, 2-phenyl-4-methylimidazoline, benzimidazole, and 1-cyanoethylimidazole.

[0080] Examples of the acid anhydride include phthalic anhydride, hexahydrophthalic anhydride, pyromellitic dianhydride, and benzophenonetetracarboxylic dianhydride.

[0081] As the organic phosphorus compound, any phosphorus compound having an organic group can be used without particular limitation, and examples thereof include hexamethylphosphoric acid triamide, tris(dichloropropyl) phosphate, tris(chloropropyl) phosphate, triphenyl phosphite, trimethyl phosphate, phenylphosphonic acid, triphenylphosphine, tri-n-butylphosphine, diphenylphosphine, and the like.

[0082] One of these curing agents may be used alone, or two or more of them may be used in combination. The amount of these curing agents may be used without particular limitation as long as the curing reaction of the epoxy group can proceed, and is preferably used in the range of 0.0 to 5.0 equivalents, particularly preferably in the range of 0.0 to 1.2 equivalents, relative to 1 mol of the epoxy group. In addition, among epoxy resins and curing agents, compounds that are not mutagenic, such as epoxy resins and curing agents that do not use bisphenol A, are preferred because they have little impact on the environment and the human body.

[0083] (Curing accelerator)

[0084] There is no particular limitation on the curing accelerator, and for example, tertiary amines, imidazoles, quaternary ammonium salts, etc. can be used. As imidazoles, for example, 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, etc. can be cited, and these substances can also be used alone or in combination of two or more. Imidazoles are sold, for example, by Shikoku Chemical Industry Co., Ltd. under the trade names of 2E4MZ, 2PZ-CN, 2PZ-CNS, and 2MA-OK.

[0085] From the perspective of extending the use period of the film, a latent curing accelerator is preferred. Representative examples thereof include dihydrazide compounds such as dicyandiamide and adipic acid dihydrazide, guanamine acid, melamine acid, addition compounds of epoxy compounds and imidazole compounds, addition compounds of epoxy compounds and dialkylamines, addition compounds of amines and thioureas, and addition compounds of amines and isocyanates. In addition, from the perspective of being able to reduce the activity at room temperature, substances having an adduct-type structure are preferred.

[0086] The amount of the curing accelerator is preferably 0 to 10.0% by mass, more preferably 0.02 to 5.0% by mass, and even more preferably 0.03 to 4.0% by mass, based on the total amount of the epoxy resin and the curing agent. If the amount of the curing accelerator exceeds 4.0% by mass, the storage stability tends to decrease and the pot life tends to be insufficient.

[0087] The total content of (c) curing agent and curing accelerator in the adhesive film is preferably more than 0 mass part and less than 5.0 mass parts, more preferably 0.02 to 3.0 mass parts, and further preferably 0.03 to 2.0 mass parts, relative to 100 mass parts of the total amount of (a) polymer, (b) epoxy resin, (c) curing agent and curing accelerator, and (d) filler. In addition, the "total content of (c) curing agent and curing accelerator" refers to the content of curing agent when the (c) component is only curing agent, and refers to the content of curing accelerator when it is only curing accelerator.

[0088] <(d) Filler>

[0089] (d) The filler has a thermal conductivity of 10 W / (m·K) or more. As the (d) filler, there can be mentioned electrical insulating materials such as aluminum oxide particles, boron nitride particles, aluminum nitride particles, silicon nitride particles, zinc oxide particles, magnesium oxide particles, aluminum hydroxide particles, magnesium hydroxide particles and diamond. One of them can be used alone, or two or more can be used in combination. Among them, aluminum oxide particles and boron nitride particles have high thermal conductivity, excellent dispersibility, and good water resistance, and are preferred from the perspective of easy availability. Among aluminum oxides, α-alumina is preferred, and its Al2O3 purity is preferably 99.90% or more, more preferably 99.92% or more, and further preferably 99.95% or more. There is no particular upper limit on the thermal conductivity. The higher the purity of the α-alumina filler, the higher the thermal conductivity. As high-purity α-alumina, Sumicorundum's AA series (manufactured by Sumitomo Chemical Industries, trade name) can be mentioned.

[0090] The average particle size (d50) of the filler (d) is preferably less than 1 / 2 of the thickness of the adhesive film, more preferably less than 1 / 3, and further preferably less than 1 / 4. When the average particle size of the filler (d) exceeds 1 / 2 of the thickness of the adhesive film, the surface irregularities of the film increase, and the bonding strength, lamination, reliability, etc. may be reduced. As the filler (d), a filler having an average particle size (d50) of one type may be used alone, or two or more fillers having different average particle sizes (d50) may be used in combination.

[0091] The content of the filler (d) in the adhesive film is preferably 60 to 95 parts by mass, more preferably 65 to 95 parts by mass, and even more preferably 70 to 90 parts by mass, relative to 100 parts by mass of the total amount of the polymer (a), the epoxy resin (b), the curing agent and the curing accelerator (c), and the filler (d). If the content of the filler (d) is less than 60 parts by mass, the thermal conductivity of the adhesive film may become insufficient, and if it exceeds 95 parts by mass, the flexibility and adhesion of the adhesive film may be reduced.

[0092] <Other ingredients>

[0093] The adhesive composition constituting the adhesive film of the present embodiment may contain, in addition to the above-mentioned components (a) to (d), for example, a curing accelerator, a filler, a coupling agent, an ion trapping agent, and a flux.

[0094] (Filling)

[0095] In order to improve the handling properties of the adhesive composition, adjust the melt viscosity, impart thixotropy, improve moisture resistance, etc., various fillers other than the filler (d) (thermal conductivity is 10 W / (m·K) or more) may be added to the resin composition. Examples of such fillers include aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum borate whiskers, crystalline silica, amorphous silica, antimony oxide, etc. Among them, in order to improve thermal conductivity, crystalline silica, amorphous silica, etc. are preferred. In order to adjust the melt viscosity or impart thixotropy, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, crystalline silica, amorphous silica, etc. are preferred. In order to improve moisture resistance, silica, aluminum hydroxide, antimony oxide are preferred. The content of these fillers is preferably 0 to 50 parts by mass, more preferably 0 to 20 parts by mass, and even more preferably 0 to 10 parts by mass, relative to 100 parts by mass of the filler (d).

[0096] (Coupling agent)

[0097] In order to improve the interface bonding between dissimilar materials, various coupling agents can also be added to the adhesive composition. As coupling agents, silane-based, titanium-based, aluminum-based, etc. can be cited, among which silane-based coupling agents are preferred. The amount of the coupling agent added is preferably 0 to 10 parts by mass relative to 100 parts by mass of the total amount of the resin component from the aspects of its effect, heat resistance and cost.

[0098] The silane coupling agent is not particularly limited, and examples thereof include vinyl trichlorosilane, vinyl tri(β-methoxyethoxy)silane, vinyl triethoxysilane, vinyl trimethoxysilane, γ-methacryloxypropyl trimethoxysilane, γ-methacryloxypropyl methyl dimethoxysilane, β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, γ-glycidyloxypropyl trimethoxysilane, γ-glycidyloxypropyl methyl dimethoxysilane, γ-glycidyloxypropyl methyl diethoxysilane, N-β-(aminoethyl)-γ-aminopropyl trimethoxysilane, N-β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, -(Aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-aminopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-ureidopropyltriethoxysilane, 3-ureidopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyl-tri(2-methoxy-ethoxy-ethoxy)silane, N-methyl-3-aminopropyltrimethoxysilane, triaminopropyl-trimethoxysilane, 3-(4,5-dihydro)imidazol-1-yl-propyl Trimethoxysilane, 3-methacryloyloxypropyl-trimethoxysilane, 3-mercaptopropyl-methyldimethoxysilane, 3-chloropropyl-methyldimethoxysilane, 3-chloropropyl-dimethoxysilane, 3-cyanopropyl-triethoxysilane, hexamethyldisilazane, N, O-bis(trimethylsilyl)acetamide, methyltrimethoxysilane, methyltriethoxysilane, ethyltrichlorosilane, n-propyltrimethoxysilane, isobutyltrimethoxysilane, amyltrichlorosilane, octyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, methyltri(methacryloyloxyethoxy)silane, methyltri (Glycidyloxy)silane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane, octadecyldimethyl[3-(trimethoxysilyl)propyl]ammonium chloride, γ-chloropropylmethyldichlorosilane, γ-chloropropylmethyldimethoxysilane, γ-chloropropylmethyldiethoxysilane, trimethylsilyl isocyanate, dimethylsilyl isocyanate, methylsilyl triisocyanate, vinylsilyl triisocyanate, phenylsilyl triisocyanate, tetraisocyanate silane, ethoxysilane isocyanate, etc., and any one of them may be used alone or in combination of two or more.

[0099] The titanium coupling agent is not particularly limited, and examples thereof include isopropyl trioctanoyl titanate, isopropyl di(methacryloyl) isostearyl titanate, isopropyl tri(dodecylbenzenesulfonyl) titanate, isopropyl isostearyl diacryloyl titanate, isopropyl tri(dioctyl phosphate) titanate, isopropyl tricumylphenyl titanate, isopropyl tri(dioctyl pyrophosphate) titanate, isopropyl tri(n-aminoethyl) titanate, tetraisopropyl bis(dioctyl phosphite) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, dicumylphenyloxy acetate titanate, bis(dioctyl pyrophosphate)oxy Acetate titanate, tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, tetra(2-ethylhexyl) titanate, titanium acetylacetonate, titanium polyacetylacetonate, titanium octanediate, ammonium titanium lactate, titanium lactate, ethyl titanium lactate, triethanolamine titanium, polyhydroxytitanium stearate, tetramethyl orthotitanate, tetraethyl orthotitanate, tetrapropyl orthotitanate, tetraisobutyl orthotitanate, stearyl titanate, cresyl titanate monomer, cresyl titanate polymer, diisopropoxy-bis(2,4-pentanedione)titanium (IV), diisopropyl-bis-triethanolamino titanate, octanediol titanate, tetra-n-butoxytitanium polymer, tri-n-butoxytitanium monostearate polymer, tri-n-butoxytitanium monostearate, and the like may be used alone or in combination of two or more.

[0100] The aluminum coupling agent is not particularly limited, and for example, aluminum acetoacetate aluminum diisopropionate, tris(ethyl acetoacetate) aluminum, alkyl acetoacetate aluminum diisopropionate, aluminum monoacetoacetate bis(ethyl acetoacetate), aluminum trisacetylacetonate, aluminum-monoisopropoxymonooleoylethyl acetoacetate, aluminum-di-n-butoxide-mono-ethyl acetoacetate, aluminum chelates such as aluminum diisopropoxide-monoethyl acetoacetate, aluminum isopropionate, mono-sec-butoxyaluminum diisopropionate, aluminum sec-butyrate, aluminum alcoholates such as aluminum acetate, and the like can be used. One of these can be used alone, or two or more of them can be used in combination.

[0101] (Ion Traps)

[0102] In order to adsorb ionic impurities so that the insulation reliability during moisture absorption becomes good, an ion capture agent can also be added to the adhesive composition. The amount of the ion capture agent is preferably 1 to 10 parts by mass relative to the total amount of 100 parts by mass of the resin component from the perspective of the effect of addition, heat resistance and cost. As an ion capture agent, a commercially available product can be appropriately selected according to the object to be captured. Compounds known as copper damage preventers for preventing copper from ionizing and dissolving, such as triazine thiol compounds, bisphenol-based reducing agents, and inorganic ion adsorbents can be used. Copper damage preventers with triazine thiol compounds as components are commercially available under the product name: ZISNET DB manufactured by Sankyo Pharmaceutical Co., Ltd. As bisphenol-based reducing agents, 2,2'-methylene-bis-(4-methyl-6-tert-butylphenol), 4,4'-thio-bis-(3-methyl-6-tert-butylphenol), etc. can be cited, and they are commercially available under the product name: YOSHINOX BB manufactured by Yoshitomi Pharmaceutical Co., Ltd. Examples of the inorganic ion adsorbent include zirconium compounds, antimony-bismuth compounds, and magnesium-aluminum compounds. IXE is commercially available from Toagosei Chemical Industry Co., Ltd.

[0103] <Manufacturing of varnish>

[0104] The solvent used when preparing the varnish is not particularly limited, and for example, methyl ethyl ketone, acetone, methyl isobutyl ketone, 2-ethoxyethanol, toluene, butyl cellosolve, methanol, ethanol, 2-methoxyethanol, dimethylacetamide, dimethylformamide, methyl pyrrolidone, cyclohexanone, etc. can be used. Among them, in order to improve the coating properties, etc., high boiling point solvents such as methyl ethyl ketone, dimethylacetamide, dimethylformamide, methyl pyrrolidone, cyclohexanone are preferred. These solvents can be used alone or in combination of two or more.

[0105] The amount of solvent is not particularly limited, but the nonvolatile component is preferably 40 to 90% by mass, more preferably 50 to 80% by mass, when preparing the varnish. When the nonvolatile component is less than 40% by mass, the amount of solvent volatilized during the preparation of the varnish is large, and a large amount of heat is required during drying, which tends to be disadvantageous in terms of cost; when it exceeds 90% by mass, the viscosity of the varnish becomes too high, so there is a possibility of defects in the coating film.

[0106] The manufacture of the varnish can be carried out by using a grinder, a triple roll, a bead mill, etc., or by combining them, taking into account the dispersibility of the filler (d) and other fillers. The time required for mixing can also be shortened by mixing the filler component and the low molecular weight substance in advance and then mixing the high molecular weight substance. In addition, after the varnish is made, it is preferred to remove the bubbles in the varnish by vacuum degassing.

[0107] <Manufacturing of adhesive film>

[0108] After the varnish is applied to the carrier film, the solvent is removed by heating, thereby forming an adhesive film on the carrier film. The heating conditions are not particularly limited as long as the solvent can be removed without completely curing the resin composition. The conditions vary depending on the components of the resin composition and the type of solvent, but generally, heating is performed at 80 to 140° C. for 5 to 60 minutes. The resin composition is preferably cured to the B stage by heating. The residual solvent content of the adhesive film is preferably 3% by mass or less, more preferably 1.5% by mass or less.

[0109] As the carrier film, a polytetrafluoroethylene film, a polyethylene terephthalate film, a polyethylene film, a polypropylene film, a polymethylpentene film, a polyimide film, a polyethylene naphthalate film, a polyethersulfone film, a polyetheramide film, a polyetheramideimide film, a polyamide film, a polyamideimide film and other plastic films can be used. In addition, a primer coating, a UV treatment, a corona discharge treatment, a grinding treatment, an etching treatment, a demolding treatment and other surface treatments can also be performed as needed. As a commercial product of the carrier film, for example, there are DuPont-Toray Co., Ltd., trade name: Kapton (polyimide film), Zhongyuan Chemical Industry Co., Ltd., trade name: Apical (polyimide film), DuPont-Toray Co., Ltd., trade name: Lumirror (polyethylene terephthalate film), Teijin Co., Ltd., trade name: Purex (polyethylene terephthalate film), etc.

[0110] <Dicing die bonding integrated film>

[0111] The adhesive film of this embodiment can be applied to, for example, a dicing die bonding integrated film. Figure 1 As shown in FIG. 1 , the dicing die bonding integrated film 30 of the present embodiment includes a die bonding film 10 formed of the above-mentioned adhesive film and a dicing film 20 laminated on the die bonding film 10 .

[0112] As the cutting film 20, for example, plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, and polyimide film can be cited. The cutting film 20 can also be subjected to surface treatments such as primer coating, UV treatment, corona discharge treatment, grinding treatment, and etching treatment as needed. The cutting film 20 preferably has adhesion, for example, a film obtained by imparting adhesion to the above-mentioned plastic film, and a film obtained by providing an adhesive layer on one side of the above-mentioned plastic film. The adhesive layer is formed, for example, by a resin composition (adhesive layer forming resin composition) containing a liquid component and a high molecular weight component and having an appropriate adhesion strength. The cutting tape with an adhesive layer can be manufactured, for example, as follows: the adhesive layer forming resin composition is applied to the above-mentioned plastic film and dried, or the adhesive layer formed by applying the adhesive layer forming resin composition to a substrate film such as a PET film and drying is pasted on the above-mentioned plastic film. The adhesion strength is set to a desired value by adjusting the ratio of the liquid component and the Tg of the high molecular weight component, for example. The chip bonding film is the adhesive film of the present embodiment described above. The dicing film and the chip bonding film may be in direct contact or may be laminated via other layers such as an adhesive layer.

[0113] The dicing die bonding integrated film 30 can be manufactured, for example, by using the dicing film 20 instead of the base film in the manufacturing method of the above-mentioned adhesive film. In addition, the dicing die bonding integrated film 30 can also be manufactured, for example, by separately preparing the die bonding film 10 and the dicing film 20 formed of the above-mentioned adhesive film, and stacking and integrating them.

[0114] Example

[0115] The present disclosure will be described in more detail below based on examples, but the present invention is not limited to these.

[0116] The following components were used in Examples and Comparative Examples.

[0117] (a) Polymer

[0118] Phenoxy resin: ZX-1356-2 (manufactured by Tohto Kasei Co., Ltd., molecular weight 63,000, ring parameter 0.59)

[0119] Epoxy-containing acrylic rubber: HTR-860P-3 (produced by Teikoku Chemical Industry Co., Ltd., molecular weight: 1 million, Tg: -7°C, ring parameter: 0.0)

[0120] (b) Epoxy resin

[0121] Bisphenol F type epoxy resin: YDF-8170C (manufactured by Tohto Kasei Co., Ltd., epoxy equivalent: 156, liquid epoxy resin, ring parameter: 0.46)

[0122] Cresol novolac type epoxy resin: YDCN-700-10 (manufactured by Tohto Kasei Co., Ltd., ring parameter: 0.40)

[0123] ·Multifunctional epoxy: 1032H60 (manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd., ring parameter 0.49)

[0124] ·YL7175-1000 (manufactured by Japan Epoxy Resin Co., Ltd., ring parameter is 0.34)

[0125] (c) Curing agent and curing accelerator

[0126] Phenolic resin (curing agent): XLC-LL (Mitsui Chemicals, Inc., ring parameter: 0.73)

[0127] Curing accelerator: Curezol 2PZ-CN (manufactured by Shikoku Chemical Industry Co., Ltd.)

[0128] Curing accelerator: Curezol 2MA-OK (manufactured by Shikoku Chemical Industry Co., Ltd.)

[0129] (d) Filling

[0130] Spherical α-alumina: Alumina beads CB-P05 (manufactured by Showa Denko K.K., Al2O3 purity 99.89%, average particle size 4 μm)

[0131] (e) Other additives:

[0132] ·A-189 (manufactured by Unicar Co., Ltd., Japan, γ-mercaptopropyltrimethoxysilane)

[0133] ·A-1160 (manufactured by Unicar Co., Ltd., γ-ureidopropyltriethoxysilane)

[0134] 2-Methylglutaric acid (manufactured by Wako Pure Chemical Industries, Ltd.)

[0135] (Example 1)

[0136] First, a composition consisting of the following ingredients was prepared.

[0137] Bisphenol F type epoxy resin: YDF-8170C (manufactured by Tohto Kasei Co., Ltd.) 4.0 parts by mass

[0138] Cresol novolac epoxy resin: YDCN-700-10 (manufactured by Tohto Kasei Co., Ltd.) 1.0 part by mass

[0139] Phenolic resin: XLC-LL (Mitsui Chemicals, Inc.) 5.5 parts by mass

[0140] ·Curezol 2PZ-CN (manufactured by Shikoku Chemical Industry Co., Ltd.) 0.01 parts by mass

[0141] A-189 (manufactured by Unicar Co., Ltd., γ-mercaptopropyltrimethoxysilane) 0.04 parts by mass

[0142] · A-1160 (γ-ureidopropyltriethoxysilane, manufactured by Unicar Co., Ltd.) 0.08 parts by mass

[0143] Cyclohexanone was added to the above composition in such a manner that the solid content reached about 80% by mass, and 85.0 parts by mass of spherical α-alumina: alumina beads CB-P05 (manufactured by Showa Denko K.K.) were further added. An equal amount (mass) of zirconium oxide beads (1 mmφ) were added to the composition, and the mixture was mixed at 600 rpm for 30 minutes using a bead mill. Phenoxy resin: 4.5 parts by mass of ZX-1356-2 (manufactured by Tohto Kasei Co., Ltd.) was added to the mixed composition, and the mixture was mixed again at 600 rpm for 30 minutes using a bead mill. After mixing, the zirconium oxide beads were removed by filtration to obtain a varnish.

[0144] As a carrier film, a 38 μm thick release-treated polyethylene terephthalate film: A53 (manufactured by Teijin Dupont Film Co., Ltd.) was prepared. After applying a varnish on the film, it was dried by heating at 120° C. for 5 minutes to prepare a 25 μm thick adhesive film on the carrier film.

[0145] (Examples 2 to 4)

[0146] Adhesive films of Examples 2 to 4 were prepared in the same manner as in Example 1 except that the blending amounts of the respective components were those shown in Table 1.

[0147] (Comparative Example 1)

[0148] First, a composition consisting of the following ingredients was prepared.

[0149] Bisphenol F type epoxy resin: YDF-8170C (manufactured by Tohto Kasei Co., Ltd.) 4.0 parts by mass

[0150] Cresol novolac epoxy resin: YDCN-700-10 (manufactured by Tohto Kasei Co., Ltd.) 1.0 part by mass

[0151] Phenolic resin: XLC-LL (Mitsui Chemicals, Inc.) 5.5 parts by mass

[0152] Curing accelerator: Curezol 2PZ-CN (manufactured by Shikoku Chemical Industry Co., Ltd.) 0.01 parts by mass

[0153] Coupling agent: A-189 (manufactured by Unicar Co., Ltd.) 0.04 parts by mass

[0154] Coupling agent: A-1160 (manufactured by Unicar Co., Ltd.) 0.08 parts by mass

[0155] Cyclohexanone was added to the above composition in such a manner that the solid content reached about 57% by mass, and 85.0 parts by mass of spherical α-alumina: alumina beads CB-P05 (manufactured by Showa Denko K.K.) were further added. An equal amount (mass) of zirconium oxide beads (1 mmφ) were added to the composition, and the mixture was mixed at 600 rpm for 30 minutes using a bead mill. 4.5 parts by mass of epoxy-containing acrylic rubber: HTR-860P-3 (manufactured by Imperial Chemical Industries, Ltd.) were added to the mixed composition, and the mixture was mixed again at 600 rpm for 30 minutes using a bead mill. After mixing, the zirconium oxide beads were removed by filtration to obtain a varnish.

[0156] As a carrier film, a 38 μm thick release-treated polyethylene terephthalate film: A31 (manufactured by Teijin Dupont Film Co., Ltd.) was prepared. After applying a varnish on the film, it was dried by heating at 120° C. for 5 minutes to prepare a 25 μm thick adhesive film on the carrier film.

[0157] (Comparative Examples 2 to 4)

[0158] Adhesive films of Comparative Examples 2 to 4 were prepared in the same manner as in Comparative Example 1 except that the blending amounts of the respective components were those shown in Table 2.

[0159] [Evaluation items]

[0160] (Thermal conductivity)

[0161] The adhesive film was attached to prepare a sample having a thickness of 100 μm or more and less than 600 μm. The sample was cured at 110° C. for 1 hour and at 170° C. for 3 hours.

[0162] Thermal diffusivity α(mm 2 / s):

[0163] The cured sample was cut into 10 mm squares to obtain a sample for measuring thermal diffusivity. The thermal diffusivity of the sample (in the thickness direction of the adhesive film) was measured at 25°C using a laser flash method (LFA467 HyperFlash manufactured by NETZSCH).

[0164] Specific heat Cp (J / (g·℃)):

[0165] The specific heat of the sample after curing was measured using the DSC method (DSC8500 manufactured by Perkin Elmer) at a temperature increase rate of 10°C / min and a temperature of 10 to 60°C to obtain a value at 25°C.

[0166] Specific gravity (g / cm 3 ):

[0167] The specific gravity of the sample after the curing was determined using an electronic densimeter SD-200L (manufactured by Mirage).

[0168] The thermal conductivity (W / (m·K)) was calculated using the following formula from the values ​​of the thermal diffusivity α, the specific heat Cp, and the specific gravity obtained in each measurement.

[0169] Thermal conductivity (W / (m·K)) = Thermal diffusivity (mm 2 / s)×specific heat (J / (g·℃))×specific gravity (g / cm 3 )

[0170] (Surface roughness Ra)

[0171] The adhesive film and a 300 μm thick silicon wafer were bonded using a heated roll laminator (80°C, 0.3 m / min, 0.3 MPa), and then cured at 110°C for 1 hour and at 170°C for 3 hours to obtain a sample. The surface roughness (Ra) of the adhesive film was determined within a range of 2.5 mm using a micro-profile measuring instrument SURFCORDER ET200 (manufactured by Kosaka Laboratory Co., Ltd.).

[0172] (Adhesion)

[0173] The adhesive film was attached to a semiconductor chip (5 mm square) using a heated roll laminator (80°C, 0.3 m / min, 0.3 MPa). The sample was then bonded to a 42 alloy substrate at 120°C and 250 g for 5 seconds, cured at 110°C for 1 hour, and cured at 170°C for 3 hours. The shear strength of the sample was measured using a universal adhesive strength tester (Dage, Series 4000).

[0174] Table 1

[0175]

[0176] Table 2

[0177]

[0178] Industrial Applicability

[0179] According to the present disclosure, it is possible to provide an adhesive film capable of achieving both adhesiveness and heat dissipation at sufficiently high levels, and a dicing die bonding integrated film including the adhesive film as a die bonding film.

[0180] Explanation of symbols

[0181] 10 Die bonding film (adhesive film)

[0182] 20 Cutting film

[0183] 30 Cutting chip bonding integrated film

Claims

1. A heat-curable die bonding film comprising: (a) polymers; (b) Epoxy resin which is liquid at 50°C; (c) at least one of a curing agent and a curing accelerator; and (d) Fillers with a thermal conductivity of 10 W / (m·K) or more, The die bonding film satisfies the condition shown in the following inequality (1), The shear strength after thermal curing is above 1.5MPa. (ma+mb+mc) / M≥0.47 (1) Wherein, ma represents the carbon mass forming the cyclic structure of (a) the polymer, mb represents the carbon mass forming the cyclic structure of (b) the epoxy resin, mc represents the carbon mass forming the cyclic structure of (c) the curing agent and the curing accelerator, and M represents the total mass of (a) the polymer, (b) the epoxy resin, and (c) the curing agent and the curing accelerator. The (a) polymer contains a phenoxy resin having a glass transition temperature Tg lower than 85°C.

2. The die bonding film according to claim 1, wherein The arithmetic mean roughness Ra of the film surface after thermal curing was 0.25 μm or less.

3. The die bonding film according to claim 1 or 2, wherein (a) The polymer includes a polymer satisfying the condition shown in the following inequality (2), at / M A ≥0.40 (2) In the formula, ma represents the carbon mass forming the ring structure of the polymer, M A Represents the total mass of the polymer.

4. The die bonding film according to claim 1 or 2, wherein (d) The filler is α-alumina particles. The die-bonding film according to claim 1 or 2, which has a thickness of 50 μm or less.

6. The die bonding film according to claim 1 or 2, wherein The content of the filler (d) is 60 to 95 parts by mass when the total amount of the (a) polymer, (b) epoxy resin, (c) curing agent and curing accelerator, and (d) filler is 100 parts by mass.

7. A dicing die bonding integrated film comprising: The die bonding film according to any one of claims 1 to 6; and A dicing film is laminated on the die-bonding film.