Processing technology of anti-aging latex mattress
A processing technology and anti-aging technology, applied in the field of mattresses, can solve the problems of latex layer performance decline, reduce original efficacy, poor anti-aging performance, etc., and achieve the effect of prolonging time, correcting bad sleeping posture, and good anti-aging performance.
Patent Information
- Authority / Receiving Office
- CN · China
- Current Assignee / Owner
- Publication Date
- 2019-11-08
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 1 
Figure 2 
Figure 3
Abstract
Description
technical field
[0001] The invention belongs to the technical field of mattresses, in particular to an aging-resistant latex mattress processing technology. Background technique
[0002] Mattress is an item between the human body and the bed to ensure consumers get a healthy and comfortable sleep. The contact area of latex mattresses is much higher than that of ordinary mattresses. Disperses the tolerance of human body weight, has the function of correcting bad sleeping positions, and has the effect of sterilizing bacteria. With the improvement of the quality of life, people hope to mix latex mattresses with bamboo charcoal. However, if the two are mixed separately for foaming, due to poor compatibility, the performance of the prepared latex layer will decrease and the original efficacy will be reduced. At the same time, the existing latex bed has poor aging resistance. Contents of the invention
[0003] The purpose of the present invention is to provide a kind of anti...
Examples
Embodiment 1
[0020] A kind of aging-resistant latex mattress processing technology, comprises the following steps:
[0021] (1) Preparation of latex layer 2: Add 3% of its mass anionic surfactant to natural latex, stir at 250r / min for 20min at 25°C, and then add 5.5% of natural latex by high-temperature steam fumigation Bamboo charcoal powder, 3% vulcanizing agent, 2% vulcanization accelerator, 1% anti-aging agent, at 30 ℃, stir 30min with 500r / min rotating speed, obtain latex dispersion liquid; The described latex dispersion that obtains The liquid is foamed, and nitrogen is passed into the latex dispersion for foaming, and a curing agent of 5.5% of the latex dispersion quality is added to obtain a foaming material, which is added to the mold and boiled for 55 minutes. Then carry out demoulding, dry and get final product, described anti-aging agent is anti-aging agent 264;
[0022] (2) Preparation of the elastic bamboo charcoal layer 3: the elastic bamboo charcoal layer 3 is composed of ...
Embodiment 2
[0032] A kind of aging-resistant latex mattress processing technology, comprises the following steps:
[0033] (1) Preparation of latex layer 2: Add 5% of its mass anionic surfactant to natural latex, stir at 250r / min for 25min at 30°C, and then add 5.8% of natural latex by high-temperature steam fumigation Bamboo charcoal powder, 4% vulcanizing agent, 3% vulcanization accelerator, 2% anti-aging agent, at 35 ℃, stir 30min with 500r / min rotating speed, obtain latex dispersion liquid; The described latex dispersion that obtains The liquid is foamed, and nitrogen is passed into the latex dispersion for foaming, and a curing agent of 6% of the latex dispersion is added to obtain a foam, which is added to the mold and boiled for 60 minutes. Then carry out demoulding, dry and get final product, described anti-aging agent is anti-aging agent 264;
[0034] (2) Preparation of the elastic bamboo charcoal layer 3: the elastic bamboo charcoal layer 3 is composed of bamboo charcoal powder...
Embodiment 3
[0044] A kind of aging-resistant latex mattress processing technology, comprises the following steps:
[0045] (1) Preparation of latex layer 2: After adding 3-5% of its mass anionic surfactant to the natural latex, stir at 250r / min for 22min at 28°C, and then add high-temperature steam passing through 5.6% of the mass of natural latex Fumigation modified bamboo charcoal powder, 3.5% vulcanizing agent, 2.5% vulcanization accelerator, 1.5% anti-aging agent, at 32°C, stirred for 30min at a speed of 500r / min to obtain a latex dispersion; the obtained The latex dispersion is foamed, and nitrogen is passed into the latex dispersion for foaming, and a curing agent of 5.6% of the latex dispersion quality is added to obtain a foaming material, which is added to the mold and boiled 58min, then carry out demoulding, dry and get final product, described anti-aging agent is anti-aging agent 264;
[0046] (2) Preparation of the elastic bamboo charcoal layer 3: the elastic bamboo charcoal la...