Interconnect structure and manufacturing method thereof, and semiconductor device
By using ruthenium tantalum as a barrier layer and protective layer in semiconductor devices, an arc-shaped through hole structure is formed, which solves the problems of copper interconnect line resistance and anti-electron migration performance, and achieves the effect of reducing RC delay and power consumption.
Patent Information
- Application Number
- CN201910024057.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-01-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2039-01-10
AI Technical Summary
As semiconductor device feature sizes shrink, the resistance of copper interconnect lines and through-hole resistance increases, causing RC delay and power consumption to worsen, while copper's anti-electromigration properties are affected.
Using a second barrier layer and a protective layer containing ruthenium tantalide, forming a second barrier layer on the sidewall and bottom of the second groove, and etching the protective layer at the bottom of the through hole to form an arc-shaped through hole, thereby enlarging the through hole current cross-sectional area, reducing contact resistance and improving resistance to electron migration.
It effectively reduces RC delay and power consumption, improves the anti-electron migration performance of copper wires, prevents the formation of opening overhangs and voids, and improves Cu plating performance.
Smart Images

Figure CN111430295B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to an interconnect structure and a manufacturing method thereof, and a semiconductor device. Background Art
[0002] In today's semiconductor industry, copper interconnects are gradually replacing aluminum interconnects. Compared with aluminum wires, copper wires have the following advantages: 1) resistivity 2) good resistance to electron migration. Copper's resistance to electron migration is higher than that of aluminum; 3) copper's melting and boiling points are higher than aluminum, and its thermal budget is better than that of aluminum.
[0003] However, copper has poor adhesion to silicon oxide and has a high diffusion rate in silicon oxide and silicon. The diffusion of copper can cause serious metal contamination. Tantalum / tantalum nitride (Ta / TaN) is generally used as a copper diffusion barrier layer in the process. Tantalum has good adhesion to copper and tantalum nitride has good diffusion barrier properties for copper.
[0004] However, as the feature size continues to shrink, the proportion of Ta / TaN in the wire cross-section becomes larger and larger. At 20°C, the resistivity of Ta film is 150-180μΩ·cm, and that of TaN is 200-240μΩ·cm, which increases the line resistance and through-hole resistance, resulting in RC delay and deterioration of power consumption. At the same time, as the feature size continues to shrink, the performance of Cu wire in resisting electron migration will be affected. Summary of the invention
[0005] The main purpose of the present invention is to provide an interconnect structure and a manufacturing method thereof, and a semiconductor device to solve the problem of defects in copper interconnect lines caused by size reduction.
[0006] To achieve the above-mentioned purpose, the present invention provides a method for manufacturing an interconnect structure, comprising: providing a substrate, a first interlayer dielectric layer is formed on the surface of the substrate, and a first metal layer is provided in the first interlayer dielectric layer; forming a second interlayer dielectric layer, the second interlayer dielectric layer covers the first interlayer dielectric layer and the first metal layer; forming a second groove in the second interlayer dielectric layer, the second groove exposes a portion of the first metal layer; forming a second barrier layer on the sidewall and bottom of the second groove, the material of the second barrier layer includes ruthenium tantalum; and filling the second metal layer in the second groove and the through hole.
[0007] Optionally, in the method for manufacturing the interconnect structure, a first groove is formed in the first interlayer dielectric layer, and the first metal layer is filled in the first groove.
[0008] Optionally, in the method for manufacturing the interconnect structure, after forming the first groove and before filling the first metal layer, it also includes: forming a first barrier layer on the sidewall and bottom of the first groove, and the material of the first barrier layer includes ruthenium tantalum.
[0009] Optionally, in the method for manufacturing the interconnect structure, the step of forming the second groove includes:
[0010] forming a plurality of third grooves in the second interlayer dielectric layer, wherein the third grooves do not expose the first metal layer;
[0011] Forming a through hole in the second dielectric layer at the bottom of the third groove until a portion of the first metal layer is exposed, and the width of the through hole is smaller than the width of the third groove;
[0012] The third groove and the through hole together form the second groove.
[0013] Optionally, in the method for manufacturing the interconnect structure, after forming the through hole and before forming the second barrier layer, the method further includes:
[0014] Forming a protective layer on the sidewall and bottom of the second groove and the sidewall of the through hole, wherein the material of the protective layer includes nitrogen-containing ruthenium tantalum;
[0015] The steps of forming the protective layer include:
[0016] forming a protective layer on the sidewalls and bottom of the third groove and the through hole;
[0017] The protection layer and the first metal layer at the bottom of the through hole are etched to form a recess in the first metal layer so that the bottom of the through hole is arc-shaped.
[0018] Optionally, in the method for manufacturing the interconnect structure, the thickness of the protection layer is less than the thickness of the second barrier layer.
[0019] Correspondingly, the present invention also provides an interconnection structure, including: a substrate; a first interlayer dielectric layer, located on the substrate, and having a first metal layer in the first interlayer dielectric layer; a second interlayer dielectric layer, covering the first interlayer dielectric layer and the first metal layer, and having a second groove formed in the second interlayer dielectric layer, the second groove exposing a portion of the first metal layer; a second barrier layer, formed on the sidewall and bottom of the second groove, and the material of the second barrier layer includes ruthenium tantalum; and a second metal layer, filling the second groove.
[0020] Optionally, in the interconnect structure, a first groove is formed in the first interlayer dielectric layer, and the first metal layer is filled in the first groove.
[0021] Optionally, the interconnect structure further includes a first barrier layer, the first barrier layer is located on the sidewall and the bottom of the first groove, and the material of the first barrier layer includes ruthenium tantalum.
[0022] Optionally, in the interconnect structure, the second groove includes: a third groove formed in the second interlayer dielectric layer, and a through hole formed in the second interlayer dielectric layer at the bottom of the third groove, the width of the through hole is smaller than the width of the second groove, and the through hole exposes a portion of the first metal layer.
[0023] Optionally, in the interconnect structure, the interconnect structure further includes a protective layer formed on the sidewalls and bottom of the third groove and the sidewalls of the through hole, and the material of the protective layer includes nitrogen-containing ruthenium tantalum.
[0024] Optionally, in the interconnect structure, the thickness of the protection layer is smaller than the thickness of the second barrier layer.
[0025] Optionally, in the interconnect structure, a recess is formed in the first metal layer so that the bottom of the through hole is arc-shaped.
[0026] Correspondingly, the present invention also provides a semiconductor device, comprising: a substrate; a first interlayer dielectric layer, located on the substrate, and having a first metal layer in the first interlayer dielectric layer; a second interlayer dielectric layer, covering the first interlayer dielectric layer and the first metal layer, and having a second groove formed in the second interlayer dielectric layer, the second groove exposing a portion of the first metal layer; a second barrier layer, formed on the sidewall and bottom of the second groove, and the material of the second barrier layer includes ruthenium tantalum; a second metal layer, filling the second groove.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] After the second groove is formed, a second barrier layer is formed on the sidewall and bottom of the second groove. The material of the second barrier layer includes ruthenium tantalum, so that the wettability of the second metal layer formed subsequently is better.
[0029] Furthermore, the second groove includes a third groove and a through hole. After a protective layer is formed on the sidewalls and bottom of the third groove and the through hole, the protective layer and the first metal layer at the bottom of the through hole are etched to form a depression in the first metal layer, so that the bottom of the through hole is arc-shaped. The second barrier layer and the bottom of the second metal layer formed subsequently are both arc-shaped, which increases the cross-sectional area of the through hole current, thereby reducing the contact resistance of the through hole and increasing the ability to resist electron migration.
[0030] Furthermore, before forming the second barrier layer, a protective layer is formed on the sidewalls and bottom of the third groove and the sidewalls of the through hole, the material of the protective layer includes nitrogen-containing ruthenium tantalum, and the material of the second barrier layer includes ruthenium tantalum. Compared with tantalum / tantalum nitride, the through-hole resistance of ruthenium tantalum / nitrogen-containing ruthenium tantalum is reduced, which can effectively reduce RC delay and power consumption; and nitrogen-containing ruthenium tantalum can effectively block the diffusion of the second metal layer, thereby improving the performance of the device.
[0031] Furthermore, compared with the wettability of tantalum and copper, the wettability of ruthenium tantalum oxide to copper is improved, so that a very thin, uniform and continuous copper seed layer can be deposited on the ruthenium tantalum oxide to prevent the formation of open overhangs, thereby avoiding the formation of voids; and, compared with tantalum / tantalum nitride, ruthenium tantalum oxide / nitrogen-containing ruthenium tantalum oxide has enhanced barrier properties to oxygen, thereby improving the anti-electron migration effect of the Cu conductor. At the same time, forming a smooth and continuous Cu seed layer on the ruthenium tantalum oxide can improve the performance of subsequent Cu electroplating.
[0032] Furthermore, the thickness of the protective layer is smaller than that of the second barrier layer. When the protective layer at the bottom of the through hole and the first metal layer are etched, the protective layer on the side wall can block the contaminants sputtered to the side wall. Its thinner thickness can reduce costs, while the second barrier layer is thicker, and only a relatively small amount of seed layer needs to be deposited on its surface to achieve electroplating, thereby preventing the formation of opening overhangs. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figures 1a to 1d A schematic cross-sectional view of each step of a method for manufacturing an interconnect structure;
[0034] Figure 2a-2b A schematic cross-sectional view of each step of a method for manufacturing an interconnect structure;
[0035] Figure 3a-3b A schematic cross-sectional view of each step of a method for manufacturing an interconnect structure;
[0036] Figure 4a-4b A schematic cross-sectional view of each step of a method for manufacturing an interconnect structure;
[0037] Figure 5 A flow chart of a method for manufacturing an interconnect structure provided by an embodiment of the present invention;
[0038] Figure 6 A schematic cross-sectional view of a substrate provided in a method for manufacturing an interconnect structure according to an embodiment of the present invention;
[0039] Figure 7 is Figure 6 A cross-sectional schematic diagram of the structure filled with a first metal layer;
[0040] Figure 8 is Figure 7 A cross-sectional schematic diagram of a second groove formed on the structure;
[0041] Fig. 9 is Figure 8 A cross-sectional schematic diagram of a protective layer formed on the structure;
[0042] Fig.10 is Fig. 9 A schematic cross-sectional view of a structure showing a recess formed in the first metal layer at the bottom of the through hole;
[0043] Fig.11 is Fig.10 A cross-sectional schematic diagram of forming a second barrier layer on the structure shown;
[0044] Fig.12 is Fig.11 A schematic cross-sectional view of forming a metal seed layer on the structure shown;
[0045] Fig.13 is Fig.12 The cross-sectional view of the structure shown is a schematic diagram of a second metal layer filled thereon.
[0046] The reference numerals are as follows:
[0047] 10-first interlayer dielectric layer; 11-first groove; 12-first barrier layer; 13-first metal layer; 14-low dielectric constant barrier layer; 15-second interlayer dielectric layer; 16-second groove; 17-through hole; 18-second barrier layer; 19-metal seed layer; 20-second metal layer; 100-first interlayer dielectric layer; 110-first groove; 120-first barrier layer; 130-first metal layer; 140-low dielectric constant barrier layer; 150-second interlayer dielectric layer; 160-second groove; 161-third groove; 162-through hole; 170-protective layer; 180-second barrier layer; 190-metal seed layer; 200-second metal layer DETAILED DESCRIPTION
[0048] Figures 1a to 1d Schematic diagram of each step of a method for making an interconnect structure. Figure 1a As shown, firstly, a first interlayer dielectric layer 10 is formed on a substrate (not shown), and the material of the first interlayer dielectric layer 10 includes silicon oxide. A first groove 11 is formed in the first interlayer dielectric layer 10 by etching, and then a first barrier layer 12 is formed. The first barrier layer 12 covers the sidewall and bottom of the first groove 11, and the material of the first barrier layer 12 includes tantalum / tantalum nitride (Ta / TaN). Next, please refer to Figure 1bAs shown, the first metal layer 13 is filled in the first groove 11. In this embodiment, one first groove 11 may be formed, or a plurality of first grooves 11 may be formed.
[0049] Next, a low dielectric constant barrier layer 14 and a second interlayer dielectric layer 15 are sequentially formed on the first interlayer dielectric layer 10 and the first metal layer 13, and a portion of the second interlayer dielectric layer 15 is etched to form a second groove 16. The low dielectric constant barrier layer 14 comprises a stacked structure composed of silicon nitride and silicon carbide, and the material of the second interlayer dielectric layer 15 comprises silicon oxide. Then, the second interlayer dielectric layer 15 and the low dielectric constant barrier layer 14 at the bottom of the second groove 16 are etched to form a through hole 17 until a portion of the first metal layer 13 is exposed. The width of the through hole 17 is smaller than the width of the second groove 16. Figure 1c Next, a second barrier layer 18 is formed on the sidewalls and bottom of the second groove 16 and the through hole 17. The material of the second barrier layer 18 includes tantalum / tantalum nitride. Figure 1d shown.
[0050] It should be noted that, in this embodiment, tantalum / tantalum nitride (Ta / TaN) refers to a stacked structure of tantalum, tantalum nitride, or tantalum and tantalum nitride, wherein tantalum nitride is formed by nitriding tantalum.
[0051] Next, a metal seed layer 19 is formed on the sidewalls and bottom of the second groove 16 and the through hole 17, and a second metal layer 20 is filled in the second groove 16 and the through hole 17 to form an interconnection structure. The material of the metal seed layer 19 is preferably copper, and the material of the second metal layer 20 is preferably copper. However, as the feature size decreases, the copper seed layer becomes too thin, which may cause the copper seed layer to agglomerate. Figure 2a As shown, the metal seed layer 19 aggregates on the second barrier layer 18, resulting in the subsequent failure to properly fill the second metal layer 20 in the through hole 17 and the second groove 16. Figure 2b That is, the copper seed layer aggregates into lumps, resulting in failure to perform normal copper electroplating filling.
[0052] However, if the copper seed layer is too thick, it will cause overhangs to form at the via opening, such as Figure 3a As shown in FIG. 1 , if the metal seed layer 19 is too thick, an overhang will be formed on the top of the side wall of the through hole 17. When the second metal layer 20 is subsequently filled, it is very easy to form a cavity in the through hole due to the sealing of the overhang. Figure 3b shown.
[0053] Please refer to Figure 4aAs shown in the figure, after normal electroplating is completed, the Ta / TaN as a barrier layer has poor barrier performance against oxygen, resulting in poor resistance to electron migration of interconnect wires, which is prone to electromigration failure. Figure 4b As shown in FIG. 1 , as the feature size is further reduced, the proportion of Ta / TaN in the wire cross section becomes larger and larger, which increases the line resistance and through-hole resistance, resulting in the deterioration of RC delay and power consumption.
[0054] Based on the above problems, the applicant provides a method for manufacturing an interconnect structure, including: providing a substrate, a first interlayer dielectric layer is formed on the surface of the substrate, a first metal layer is provided in the first interlayer dielectric layer, a second interlayer dielectric layer is formed, the second interlayer dielectric layer covers the first interlayer dielectric layer and the first metal layer, a second groove is formed in the second dielectric layer, the second groove exposes a portion of the first metal layer, a second barrier layer is formed on the sidewall and bottom of the second groove, the material of the second barrier layer includes ruthenium tantalum, and a second metal layer is filled in the second groove.
[0055] The applicant also provides an interconnect structure, comprising: a substrate, a first interlayer dielectric layer, located on the substrate, and having a first metal layer in the first interlayer dielectric layer; a second interlayer dielectric layer, covering the first interlayer dielectric layer and the first metal layer, and having a second groove formed in the second interlayer dielectric layer, the second groove exposing a portion of the first metal layer; a second barrier layer, formed on the sidewall and bottom of the second groove, and the material of the second barrier layer includes ruthenium tantalum; and a second metal layer, filling the second groove.
[0056] In the interconnect structure and manufacturing method thereof provided by the present invention, after forming the second groove, a second barrier layer is formed on the sidewall and bottom of the second groove, and the material of the second barrier layer includes ruthenium tantalum, so that the wettability of the subsequently formed second metal layer is better.
[0057] To make the content of the present invention more clear and understandable, the content of the present invention is further described below in conjunction with the accompanying drawings. Of course, the present invention is not limited to this specific embodiment, and general replacements known to those skilled in the art are also covered within the protection scope of the present invention.
[0058] Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Secondly, the present invention is described in detail using schematic diagrams. When describing the examples of the present invention in detail, for the sake of convenience, the schematic diagrams are not partially enlarged according to general proportions, and this should not be used as a limitation of the present invention.
[0059] Please refer to Figure 5 , which is a flow chart of a method for manufacturing an interconnect structure provided by an embodiment of the present invention. Figure 5 As shown, the method for manufacturing the interconnection structure comprises the following steps:
[0060] Step S01: providing a substrate, on which a first interlayer dielectric layer is formed, and in which a first metal layer is provided;
[0061] Step S02: forming a second interlayer dielectric layer, wherein the second interlayer dielectric layer covers the first interlayer dielectric layer and the first metal layer;
[0062] Step S03: forming a plurality of second grooves in the second dielectric layer, wherein the second grooves expose a portion of the first metal layer;
[0063] Step S04: forming a second barrier layer on the sidewall and bottom of the second groove, wherein the material of the second barrier layer includes ruthenium tantalum;
[0064] Step S05: filling the second groove with a second metal layer.
[0065] Figure 6 FIG. 1 is a cross-sectional schematic diagram of a substrate provided in a method for manufacturing an interconnect structure according to an embodiment of the present invention. Figure 6 As shown, in step S01 , a substrate is provided, a first interlayer dielectric layer 100 is formed on a surface of the substrate, and a first metal layer 130 is provided in the first interlayer dielectric layer 100 .
[0066] Specifically, first, a substrate (not shown) is provided, and the material of the substrate can be single crystal silicon, polycrystalline silicon, amorphous silicon, silicon germanium compound or silicon on insulator (SOI), etc., or can be compounds such as gallium arsenide or gallium nitride, or other materials known to those skilled in the art. A semiconductor device layer (not shown) can also be formed on the surface of the substrate, and a number of semiconductor devices such as MOS field effect transistors, diodes or resistors are formed in the semiconductor device layer. These semiconductor devices need to be electrically connected through an interconnection structure composed of multi-layer conductive plugs and multi-layer metal interconnection lines to complete the electrical functions of the integrated circuit chip.
[0067] Then, a first interlayer dielectric layer 100 is formed on the substrate, for example, by a deposition process. The material of the first interlayer dielectric layer 100 includes but is not limited to silicon oxide, silicon nitride or silicon oxynitride, etc. In this embodiment, the material of the first interlayer dielectric layer 100 is preferably silicon oxide.
[0068] Next, a photoresist layer (not shown) is formed on the first interlayer dielectric layer 100, for example, it can be formed by spin coating. Then, the photoresist layer is exposed and developed to form a patterned photoresist layer, and a plurality of openings exposing the first interlayer dielectric layer 100 are formed in the patterned photoresist layer. Next, the first interlayer dielectric layer 100 is etched using the patterned photoresist layer as a mask to form a first groove 110. The depth of the first groove 110 is between 170nm and 270nm, and the width of the first groove 110 is between 70nm and 170nm. In this embodiment, one first groove 110 can be formed, or a plurality of first grooves 110 can be formed.
[0069] In this embodiment, before forming the first interlayer dielectric layer 100, it may also include: forming a third interlayer dielectric layer (not shown) on the substrate, and forming a plurality of through holes in the third interlayer dielectric layer by photolithography and etching processes to expose the area in the substrate that needs electrical connection (not shown). Then, a conductive material layer is formed on the third interlayer dielectric layer, and the conductive material fills the through hole, and the conductive material layer is planarized until the third interlayer dielectric layer is exposed to form a conductive plug located in the through hole. The material of the conductive plug includes but is not limited to tungsten, copper or cobalt. In this embodiment, the material of the conductive plug is preferably tungsten. The conductive plug connects the area in the substrate that needs electrical connection with the interconnection structure to achieve interconnection. Before forming the conductive material layer, it also includes: forming a barrier layer on the sidewall and bottom of the through hole, and the barrier layer is used to prevent the diffusion or migration of the metal in the conductive plug.
[0070] Figure 7 is Figure 6 For a cross-sectional diagram of the structure filled with the first metal layer, please refer to Figure 6 and Figure 7 As shown, a first barrier layer 120 is formed on the sidewall and bottom of the first groove 110 , and a first metal layer 130 is filled in the first groove 110 . The material of the first barrier layer 120 includes ruthenium tantalum (RuTa).
[0071] For details, please refer to Figure 6 As shown, a first barrier layer 120 is formed on the first interlayer dielectric layer 100, and the first barrier layer 120 covers the top of the first interlayer dielectric layer 100, and the sidewalls and bottom of the first groove 110. The material of the first barrier layer 120 includes but is not limited to ruthenium tantalate, and the first barrier layer 120 can be deposited on the surface of the first interlayer dielectric layer 100 and the first groove 110 by using a physical vapor deposition process but is not limited to it.
[0072] In this embodiment, the material of the target used to form the first barrier layer 120 includes 5at% to 20at% tantalum and 95at% to 80at% ruthenium, for example, the material of the target includes 10at% tantalum and 90at% ruthenium. The thickness of the first barrier layer 120 is between 10nm and 20nm, and the film resistivity of the first barrier layer 120 is 50 to 70μΩ·cm, which is much lower than the resistivity of tantalum 150 to 180μΩ·cm and the resistivity of tantalum nitride 200 to 240μΩ·cm, which can reduce the resistance of the first metal layer formed subsequently. In other embodiments, the material of the first barrier layer 120 can also be nitrogen-containing ruthenium tantalate (RuTaN), or the first barrier layer 120 can also be a stacked structure of ruthenium tantalate and nitrogen-containing ruthenium tantalate.
[0073] Next, please refer to Figure 7 As shown, a first metal layer 130 is formed, for example, by electroplating. The first metal layer 130 fills the first groove 110 and covers the first interlayer dielectric layer 100, and then the first metal layer 130 is planarized until the first interlayer dielectric layer 100 is exposed to form a first metal interconnection line. The material of the first metal layer 130 includes but is not limited to copper.
[0074] The resistivity of copper is 1.678μΩ·cm, which is lower than that of aluminum (2.65μΩ·cm). The melting and boiling points of copper are 1084.77℃ and 5555℃, respectively, which are higher than the melting and boiling points of aluminum (666℃ and 2519℃). Copper has stronger resistance to electron migration than aluminum. Compared with aluminum wires, using copper wires can significantly reduce wire resistance and improve the reliability and integration density of interconnect wires.
[0075] Please refer to Figure 8 As shown, in step S02 , a second interlayer dielectric layer 150 is formed, and the second interlayer dielectric layer 150 covers the first interlayer dielectric layer 100 and the first metal layer 130 .
[0076] Specifically, first, a low dielectric constant barrier layer 140 is formed, for example, by a deposition process, and the low dielectric constant barrier layer 140 covers the first interlayer dielectric layer 100, the first barrier layer 120, and the first metal layer 130. The material of the low dielectric constant barrier layer 140 includes but is not limited to silicon oxide, silicon nitride, silicon oxynitride, or silicon carbide nitride. In this embodiment, the low dielectric constant barrier layer 140 is a stacked structure including silicon nitride and silicon carbide nitride. The thickness of the low dielectric constant barrier layer 140 is between 60nm and 100nm.
[0077] Next, a second interlayer dielectric layer 150 is formed, for example, by a deposition process, and the second interlayer dielectric layer 150 covers the low dielectric constant barrier layer 140. The material of the second interlayer dielectric layer 150 includes but is not limited to silicon oxide, silicon nitride or silicon oxynitride, etc. In this embodiment, the material of the second interlayer dielectric layer 150 is preferably silicon oxide.
[0078] Figure 8 is Figure 7 Please refer to the cross-sectional diagram of the second groove formed on the structure. Figure 8 As shown, in step S03 , a second groove 160 is formed in the second dielectric layer 150 , and the second groove 160 exposes a portion of the first metal layer 130 .
[0079] In this embodiment, the second groove 160 includes a third groove 161 formed in the second interlayer dielectric layer 150 and a through hole 162 formed in the second dielectric layer 150 at the bottom of the third groove 161, the through hole 162 exposes a portion of the first metal layer 130, and the width of the through hole 162 is smaller than the width of the third groove 161.
[0080] Specifically, a first photoresist layer (not shown) is formed on the second interlayer dielectric layer 150, and the first photoresist layer is exposed and developed to form a first photolithography pattern, and the opening of the first photolithography pattern defines the opening width of the third groove 161 formed in the subsequent step. Then, the second interlayer dielectric layer 150 is etched according to the first photolithography pattern to form the third groove 161. The third groove 161 is located in the second interlayer dielectric layer 150 and does not penetrate the second interlayer dielectric layer 150. Then, after the first photolithography pattern is stripped, a second photoresist layer is formed, and the second photoresist layer is exposed and developed to form a second photolithography pattern, and the opening of the second photolithography pattern defines the opening width of the through hole 162 formed in the subsequent step, and the opening of the second photolithography pattern is located in the second groove 160. Next, the second interlayer dielectric layer 150 in the third groove 161 is etched according to the second photolithography pattern until the low dielectric constant barrier layer 140 is exposed, and then the low dielectric constant barrier layer 140 is etched until a portion of the first metal layer 130 is exposed, thereby forming a through hole 162. Finally, the second photolithography pattern is stripped off. The third groove 161 and the through hole 162 together constitute the second groove 160.
[0081] In this embodiment, the width of the through hole 162 is smaller than the width of the third groove 161. The depth of the through hole 162 is between 280nm and 380nm, and the width of the through hole 162 is between 50nm and 150nm; the depth of the third groove 161 is between 300nm and 500nm, and the width of the third groove 161 is between 150nm and 300nm.
[0082] Of course, in other embodiments, the through hole 162 may be formed first and then the third groove 161 may be formed. This may be determined according to actual process conditions, and the present invention is not limited thereto.
[0083] Fig. 9 is Figure 8 A schematic cross-sectional view of a protective layer formed on the structure, Fig.10 is Fig. 9 The structure shown is a cross-sectional schematic diagram of a recess formed in the first metal layer at the bottom of the through hole, Fig.11 is Fig.10 A cross-sectional diagram of a second barrier layer formed on the structure shown in FIG. Figures 9 to 11 As shown, in step S04 , a second barrier layer 190 is formed on the sidewall and the bottom of the second groove 160 , and the material of the second barrier layer 190 includes ruthenium tantalum.
[0084] In this embodiment, a protective layer 170 is first formed on the sidewalls and bottom of the third groove 161 and the sidewalls of the through hole 162, and then a second barrier layer 190 is formed on the sidewalls and bottom of the third groove 161 and the through hole 162. The material of the protective layer 170 includes nitrogen-containing ruthenium tantalum (RuTaN), and the material of the second barrier layer 190 includes ruthenium tantalum.
[0085] First, please refer to Fig. 9 As shown, a protective layer 170 is formed, for example, by a physical vapor deposition process, and the protective layer 170 covers the sidewalls and bottom of the third groove 161 and the through hole 162. The material of the protective layer 170 includes but is not limited to nitrogen-containing ruthenium tantalum. In physical vapor deposition, the material of the target material includes 10% tantalum and 90% ruthenium, the ratio of nitrogen to argon in the sputtering gas is 1:1, the bias power is 500w~1200w, and the temperature of the chamber is between 350℃ and 450℃, for example, the temperature of the chamber is 400℃. Of course, in other embodiments, the material of the protective layer 170 can also be ruthenium tantalum, or the protective layer 170 can also be a stacked structure of ruthenium tantalum and nitrogen-containing ruthenium tantalum.
[0086] Next, please refer to Fig.10As shown, the bias power is increased to 1000W-1800W, so that the argon ions in the chamber are accelerated vertically downward, and the bottom of the through hole 162 is physically etched to etch the protective layer 170 and the first metal layer 130 at the bottom of the through hole 162, and a depression is formed in the first metal layer 130, so that the bottom of the through hole 162 is arc-shaped. A small amount of Cu at the bottom of the through hole 162 will be splashed back to the side wall of the through hole 162, and will not diffuse into the second interlayer dielectric layer 150 to cause pollution. The temperature of the chamber remains unchanged during the physical etching, that is, between 350℃ and 450℃, for example, 400℃. Nitrogen-containing ruthenium tantalum has good wettability with copper sputtered onto the side wall, and copper can cover the nitrogen-containing ruthenium tantalum on the side wall of the through hole 162 well to prevent copper from diffusing into the second interlayer dielectric layer 150 to cause pollution.
[0087] Finally, the second barrier layer 180 is formed, for example, it can be formed by a physical vapor deposition process, and the second barrier layer 180 covers the sidewalls and bottom of the third groove 161 and the through hole 162. The material of the second barrier layer 180 includes but is not limited to ruthenium tantalum. In physical vapor deposition, the material of the target material is 5at% to 20at% tantalum and 95at% to 80at% ruthenium, for example, 10% tantalum and 90% ruthenium, the bias power is 500w to 1200w, and the temperature of the chamber is between 350℃ and 450℃, for example, the temperature of the chamber is 400℃. The second barrier layer 180 serves as a barrier layer and a wetting layer for the metal seed layer formed subsequently, and the thickness of the second barrier layer 180 is between 8nm and 13nm. In other embodiments, the material of the second barrier layer 180 may also be ruthenium tantalum oxide containing nitrogen (RuTaN), or the second barrier layer 180 may also be a stacked structure of ruthenium tantalum oxide and ruthenium tantalum oxide containing nitrogen.
[0088] In this embodiment, the thickness of the protective layer 170 is less than the thickness of the second barrier layer 180. When the protective layer 170 and the first metal layer 130 at the bottom of the through hole 162 are etched, the protective layer 170 on the side wall can block the contaminants sputtered to the side wall. Its thinner thickness can reduce costs, while the second barrier layer 180 is thicker, and only a relatively small amount of seed layer needs to be deposited on its surface to achieve electroplating, thereby preventing the formation of opening overhangs.
[0089] Fig.12 is Fig.11 A schematic cross-sectional view of forming a metal seed layer on the structure shown in FIG. Fig.13 is Fig.12 A cross-sectional schematic diagram of a structure filled with a second metal layer. Fig.12 and Fig.13 As shown, in step S05 , the second metal layer 210 is filled in the second groove 160 .
[0090] First, please refer to Fig.12 As shown, a metal seed layer 190 is formed on the sidewalls and bottom of the third groove 161 and the through hole 162, for example, by a physical vapor deposition process, and the metal seed layer 190 covers the second barrier layer 180. The material of the metal seed layer 190 includes but is not limited to copper.
[0091] Compared with the wettability of tantalum and copper, the wettability of ruthenium tantalum oxide to copper is improved, so that a thin copper seed layer can be formed uniformly and continuously on the ruthenium tantalum oxide (i.e., the second barrier layer 180) without agglomeration, and no overhangs will be formed at the opening due to the excessive thickness of the seed layer, so that the anti-electron migration effect of the second metal layer formed subsequently is improved, and the formation of a smooth and continuous copper seed layer on the ruthenium tantalum oxide can improve the performance of the subsequent second metal layer electroplating. The thickness of the metal seed layer 190 is between 15nm and 25nm.
[0092] Next, please refer to Fig.13 As shown, a second metal layer 200 is formed, for example, by electroplating. The second metal layer 200 fills the third groove 161 and the through hole 162 and covers the second interlayer dielectric layer 150. Then, the second metal layer 200 is planarized until the second interlayer dielectric layer 150 is exposed to form a second metal interconnection line. The material of the second metal layer 200 includes but is not limited to copper.
[0093] In this embodiment, the material of the protective layer 170 includes nitrogen-containing ruthenium tantalate, and the material of the second barrier layer 180 includes ruthenium tantalate. In other embodiments, the material of the protective layer 170 may also be ruthenium tantalate, and the material of the second barrier layer 180 may also be ruthenium tantalate containing nitrogen. Compared with tantalum / tantalum nitride, the through-hole resistance of ruthenium tantalate / nitrogen-containing ruthenium tantalate is reduced, which can effectively reduce RC delay and power consumption; and nitrogen-containing ruthenium tantalate can effectively block the diffusion of the second metal layer 200, thereby improving the performance of the device.
[0094] Moreover, compared with the wettability of tantalum and copper, the wettability of ruthenium tantalum oxide with copper is improved, so that a very thin, uniform and continuous copper seed layer can be deposited on ruthenium tantalum oxide to prevent the formation of open overhangs, thereby avoiding the formation of voids; and, compared with tantalum / tantalum nitride, ruthenium tantalum oxide / nitrogen-containing ruthenium tantalum oxide has enhanced barrier properties to oxygen, thereby improving the anti-electron migration effect of the Cu conductor. At the same time, forming a smooth and continuous Cu seed layer on ruthenium tantalum oxide can improve the performance of subsequent Cu electroplating.
[0095] Furthermore, after forming a protective layer 170 on the side walls and the bottom of the third groove 161 and the through hole 162, the protective layer 170 and the first metal layer 130 at the bottom of the through hole 162 are etched to form a depression in the first metal layer 130, so that the bottom of the through hole 162 is arc-shaped, and the bottoms of the subsequently formed second barrier layer 180, metal seed layer 180 and second metal layer 200 are all arc-shaped, which increases the cross-sectional area of the through hole current, thereby reducing the contact resistance of the through hole and increasing the ability to resist electron migration.
[0096] Of course, after forming the second metal layer 200 , the third metal layer, the fourth metal layer, etc. may be formed by the same method, which may be determined according to actual needs, and the present invention is not limited to this.
[0097] Accordingly, the present invention also provides an interconnection structure, which is manufactured using the above-mentioned interconnection structure manufacturing method. Fig.13 As shown, the interconnect structure includes: a substrate (not shown), a first interlayer dielectric layer 100, a first metal layer 130, a second interlayer dielectric layer 150, a second barrier layer 180 and a second metal layer 200. The first interlayer dielectric layer 100 is located on the substrate, and the first interlayer dielectric layer 100 has the first metal layer 130. The second interlayer dielectric layer 150 covers the first interlayer dielectric layer 100 and the first metal layer 130, and a second groove 160 is formed in the second interlayer dielectric layer 150, and the second groove 160 exposes a portion of the first metal layer 130. The second barrier layer 180 is formed on the sidewall and bottom of the second groove 160, and the material of the second barrier layer 180 includes ruthenium tantalum. The second metal layer 200 is filled in the second groove 160.
[0098] In this embodiment, a first groove 110 is formed in the first interlayer dielectric layer 100, and the first metal layer 130 is filled in the first groove 110. The number of the first groove 110 may be one or more, which is not limited in this embodiment.
[0099] In this embodiment, the second groove 160 includes: a third groove 161 formed in the second interlayer dielectric layer 150, and a through hole 162 formed in the second interlayer dielectric layer 150 at the bottom of the third groove 161, the width of the through hole 162 is smaller than the width of the second groove 161, and the through hole 162 exposes a portion of the first metal layer 130.
[0100] The interconnect structure further includes a protection layer 170 . The protection layer 170 is formed on the sidewall and bottom of the third groove 161 and the sidewall of the through hole 162 . The material of the protection layer 170 includes nitrogen-containing ruthenium tantalum.
[0101] In this embodiment, the thickness of the protective layer 170 is less than that of the second barrier layer 180. When the protective layer 170 and the first metal layer 130 at the bottom of the through hole 162 are etched, the protective layer 170 on the side wall can block the contaminants sputtered to the side wall. Its thinner thickness can reduce costs, while the second barrier layer 180 is thicker, and only a relatively small amount of seed layer needs to be deposited on its surface to achieve electroplating, thereby preventing the formation of opening overhangs.
[0102] In this embodiment, the material of the protective layer 170 includes nitrogen-containing ruthenium tantalate, and the material of the second barrier layer 180 includes ruthenium tantalate. In other embodiments, the material of the protective layer 170 may also be ruthenium tantalate, and the material of the second barrier layer 180 may also be ruthenium tantalate containing nitrogen. Compared with tantalum / tantalum nitride, the through-hole resistance of ruthenium tantalate / nitrogen-containing ruthenium tantalate is reduced, which can effectively reduce RC delay and power consumption; and nitrogen-containing ruthenium tantalate can effectively block the diffusion of the second metal layer 200, thereby improving the performance of the device.
[0103] Moreover, compared with the wettability of tantalum and copper, the wettability of ruthenium tantalum oxide with copper is improved, so that a very thin, uniform and continuous copper seed layer can be deposited on ruthenium tantalum oxide to prevent the formation of open overhangs, thereby avoiding the formation of voids; and, compared with tantalum / tantalum nitride, ruthenium tantalum oxide / nitrogen-containing ruthenium tantalum oxide has enhanced barrier properties to oxygen, thereby improving the anti-electron migration effect of the Cu conductor. At the same time, forming a smooth and continuous Cu seed layer on ruthenium tantalum oxide can improve the performance of subsequent Cu electroplating.
[0104] In this embodiment, a depression is formed in the first metal layer 130 so that the bottom of the through hole 162 is arc-shaped, and the bottoms of the second barrier layer 180 and the second metal layer 200 are both arc-shaped, thereby increasing the cross-sectional area of the through hole current, thereby reducing the contact resistance of the through hole and increasing the ability to resist electron migration.
[0105] The interconnect structure further includes: a metal seed layer 190 , wherein the metal seed layer 190 is formed on the sidewalls and the bottom of the third groove 161 and the through hole 162 ; and the metal seed layer 190 covers the second barrier layer 180 .
[0106] The interconnect structure further includes a low dielectric constant barrier layer 140 , which covers the first interlayer dielectric layer 100 , the first barrier layer 120 and the first metal layer 130 , and the second interlayer dielectric layer 150 covers the low dielectric constant barrier layer 140 .
[0107] In this embodiment, the depth of the first groove 110 is between 170nm and 270nm, and the width of the first groove 110 is between 70nm and 170nm. The depth of the through hole 162 is between 280nm and 380nm, and the width of the through hole 162 is between 50nm and 150nm. The depth of the third groove 161 is between 300nm and 500nm, and the width of the third groove 161 is between 150nm and 300nm. The thickness of the first barrier layer 120 is between 10nm and 20nm, the thickness of the protective layer 170 is between 4nm and 7nm, the thickness of the second barrier layer 180 is between 8nm and 13nm, and the thickness of the metal seed layer 190 is between 15nm and 25nm.
[0108] In this embodiment, the materials of the first interlayer dielectric layer 100 and the second interlayer dielectric layer 150 include but are not limited to silicon oxide, the materials of the first metal layer 130 and the second metal layer 200 include but are not limited to copper, the material of the metal seed layer 190 includes copper, and the material of the low dielectric constant barrier layer 140 includes silicon nitride and silicon carbide.
[0109] Accordingly, the present invention also provides a semiconductor device comprising the interconnection structure as described above.
[0110] Specifically, the semiconductor device includes: a substrate, a first interlayer dielectric layer, a first metal layer, a second interlayer dielectric layer, a second barrier layer and a second metal layer. The first interlayer dielectric layer is located on the substrate, and the first interlayer dielectric layer has the first metal layer. The second interlayer dielectric layer covers the first interlayer dielectric layer and the first metal layer, and a second groove is formed in the second interlayer dielectric layer, and the second groove exposes a portion of the first metal layer. The second barrier layer is formed on the sidewall and bottom of the second groove, and the material of the second barrier layer includes ruthenium tantalum. The second metal layer is filled in the second groove.
[0111] A depression is formed in the first metal layer so that the bottom of the through hole is arc-shaped.
[0112] To sum up, in the interconnect structure and its manufacturing method, and the semiconductor device provided by the present invention, after the second groove is formed, a second barrier layer is formed on the sidewall and bottom of the second groove, and the material of the second barrier layer includes ruthenium tantalum, so that the wettability of the subsequently formed second metal layer is better.
[0113] Furthermore, the second groove includes a third groove and a through hole. After a protective layer is formed on the sidewalls and bottom of the third groove and the through hole, the protective layer and the first metal layer at the bottom of the through hole are etched to form a depression in the first metal layer, so that the bottom of the through hole is arc-shaped. The second barrier layer and the bottom of the second metal layer formed subsequently are both arc-shaped, which increases the cross-sectional area of the through hole current, thereby reducing the contact resistance of the through hole and increasing the ability to resist electron migration.
[0114] Furthermore, before forming the second barrier layer, a protective layer is formed on the sidewalls and bottom of the third groove and the sidewalls of the through hole, the material of the protective layer includes nitrogen-containing ruthenium tantalum, and the material of the second barrier layer includes ruthenium tantalum. Compared with tantalum / tantalum nitride, the through-hole resistance of ruthenium tantalum / nitrogen-containing ruthenium tantalum is reduced, which can effectively reduce RC delay and power consumption; and nitrogen-containing ruthenium tantalum can effectively block the diffusion of the second metal layer, thereby improving the performance of the device.
[0115] Furthermore, compared with the wettability of tantalum and copper, the wettability of ruthenium tantalum oxide to copper is improved, so that a very thin, uniform and continuous copper seed layer can be deposited on the ruthenium tantalum oxide to prevent the formation of open overhangs, thereby avoiding the formation of voids; and, compared with tantalum / tantalum nitride, ruthenium tantalum oxide / nitrogen-containing ruthenium tantalum oxide has enhanced barrier properties to oxygen, thereby improving the anti-electron migration effect of the Cu conductor. At the same time, forming a smooth and continuous Cu seed layer on the ruthenium tantalum oxide can improve the performance of subsequent Cu electroplating.
[0116] Furthermore, the thickness of the protective layer is smaller than that of the second barrier layer. When the protective layer at the bottom of the through hole and the first metal layer are etched, the protective layer on the side wall can block the contaminants sputtered to the side wall. Its thinner thickness can reduce costs, while the second barrier layer is thicker, and only a relatively small amount of seed layer needs to be deposited on its surface to achieve electroplating, thereby preventing the formation of opening overhangs.
[0117] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of protection of the claims.
Claims
1. A method for manufacturing an interconnect structure, characterized in that: include: Providing a substrate, wherein a first interlayer dielectric layer is formed on the surface of the substrate, and a first metal layer is provided in the first interlayer dielectric layer; forming a second interlayer dielectric layer, wherein the second interlayer dielectric layer covers the first interlayer dielectric layer and the first metal layer; forming a second groove in the second interlayer dielectric layer, wherein the second groove exposes a portion of the first metal layer; forming a second barrier layer on the sidewall and bottom of the second groove, wherein the material of the second barrier layer includes ruthenium tantalum; as well as, Filling a second metal layer in the second groove; wherein the step of forming the second groove comprises: forming a plurality of third grooves in the second interlayer dielectric layer; forming a through hole in the second interlayer dielectric layer at the bottom of the third groove until a portion of the first metal layer is exposed, and the width of the through hole is smaller than the width of the third groove; The third groove and the through hole together constitute the second groove; After forming the through hole and before forming the second barrier layer, the method further includes: A protective layer is formed on the sidewalls and bottom of the through hole and the third groove, and the protective layer and the first metal layer at the bottom of the through hole are etched to form a recess in the first metal layer so that the bottom of the through hole is arc-shaped. The material of the protective layer includes nitrogen-containing ruthenium tantalum.
2. The method for manufacturing an interconnection structure according to claim 1, characterized in that: A first groove is formed in the first interlayer dielectric layer, and the first metal layer is filled in the first groove.
3. The method for manufacturing an interconnection structure according to claim 2, characterized in that: After forming the first groove and before filling the first metal layer, the method further includes: forming a first barrier layer on the sidewall and bottom of the first groove, wherein the material of the first barrier layer includes ruthenium tantalum.
4. The method for manufacturing an interconnection structure according to claim 1, wherein: The thickness of the protection layer is smaller than the thickness of the second barrier layer.
5. An interconnection structure, characterized in that: include: substrate; A first interlayer dielectric layer is located on the substrate, and a first metal layer is provided in the first interlayer dielectric layer; a second interlayer dielectric layer, covering the first interlayer dielectric layer and the first metal layer, wherein a second groove is formed in the second interlayer dielectric layer, wherein the second groove exposes a portion of the first metal layer, wherein the second groove comprises: a third groove formed in the second interlayer dielectric layer, and a through hole formed in the second interlayer dielectric layer at the bottom of the third groove, wherein the width of the through hole is smaller than the width of the second groove, and wherein the through hole exposes a portion of the first metal layer; A second barrier layer is formed on the sidewall and bottom of the second groove, and the material of the second barrier layer includes ruthenium tantalum; and, A second metal layer is filled in the second groove; The interconnection structure further includes a protection layer formed on the sidewall and bottom of the third groove and the sidewall of the through hole, and the material of the protection layer includes nitrogen-containing ruthenium tantalum.
6. The interconnect structure according to claim 5, characterized in that A first groove is formed in the first interlayer dielectric layer, and the first metal layer is filled in the first groove.
7. The interconnect structure according to claim 6, wherein: The invention also includes a first barrier layer, which is located on the sidewall and the bottom of the first groove, and the material of the first barrier layer includes ruthenium tantalum.
8. The interconnect structure according to claim 5, characterized in that The thickness of the protection layer is smaller than the thickness of the second barrier layer.
9. The interconnect structure according to claim 5, characterized in that A depression is formed in the first metal layer so that the bottom of the through hole is arc-shaped.
10. The interconnect structure according to claim 5, characterized in that The second barrier layer is formed by a physical vapor deposition process. In the physical vapor deposition process, a target material is used that contains 5 at% to 20 at% of tantalum and 95 at% to 80 at% of ruthenium.
11. The interconnect structure according to claim 7, wherein: The first barrier layer is formed by a physical vapor deposition process. In the physical vapor deposition process, a target material is used that contains 5 at% to 20 at% of tantalum and 95 at% to 80 at% of ruthenium.
12. The interconnect structure according to claim 5, characterized in that The ruthenium tantalum is RuTa.
13. The interconnect structure according to claim 5, characterized in that The nitrogen-containing ruthenium tantalum is RuTaN.
14. The interconnect structure according to claim 7, wherein: The interconnect structure further includes a low dielectric constant barrier layer, and the low dielectric constant barrier layer is located between the first interlayer dielectric layer and the second interlayer dielectric layer.
15. The interconnect structure according to claim 14, characterized in that The low dielectric constant barrier layer also covers the first barrier layer and a portion of the surface of the first metal layer, and the second interlayer dielectric layer covers the low dielectric constant barrier layer.
16. A semiconductor device, characterized in that: include: substrate; A first interlayer dielectric layer is located on the substrate, and a first metal layer is provided in the first interlayer dielectric layer; a second interlayer dielectric layer, covering the first interlayer dielectric layer and the first metal layer, wherein a second groove is formed in the second interlayer dielectric layer, wherein the second groove exposes a portion of the first metal layer, wherein the second groove comprises: a third groove formed in the second interlayer dielectric layer, and a through hole formed in the second interlayer dielectric layer at the bottom of the third groove, wherein the width of the through hole is smaller than the width of the second groove, and wherein the through hole exposes a portion of the first metal layer; A second barrier layer is formed on the sidewall and bottom of the second groove, and the material of the second barrier layer includes ruthenium tantalum; A second metal layer is filled in the second groove; The semiconductor device further comprises a protection layer formed on the sidewall and bottom of the third groove and the sidewall of the through hole, and the material of the protection layer comprises nitrogen-containing ruthenium tantalum.