A mixed color epitaxial structure and manufacturing method
By designing a color-mixed epitaxial structure in LEDs, using the cyclic stacked GaN layer and InxGa(1-x)N and AlyInzGa(1-y-z)N layers, electron mobility is enhanced, and the problem of insufficient electron migration in white LEDs is solved. The mixing of blue and green light is achieved, the control circuit is simplified, the cost is reduced, and the carrier concentration and current expansion is improved.
Patent Information
- Application Number
- CN202010708258.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-22
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-07-22
AI Technical Summary
In the prior art, in the implementation method of white light LED, the control circuit of RGB three-primary color mixed light is complex and costly, and the electron migration is insufficient, so it is impossible to simply mix and generate white light.
Design a color-mixed epitaxial structure, including a sequentially grown base layer, a buffer layer, a first luminescent layer, a transition layer of a superlattice structure and a second luminescent layer, through the cyclic stacked GaN layer, InxGa(1-x)N and AlyInzGa(1-y-z) N layer forms a gradient thickness gradient, enhances electron mobility, realizes the mixing of blue and green light, generates a green LED, and mixes it with red LED to generate white light.
By enhancing electron mobility, simplifying the control circuit, and reducing the cost by about 20% to 50%, the epitaxial structure of LED color display is realized, and the carrier concentration and current expansion are improved.
Smart Images

Figure CN111725366B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a structural design and a manufacturing method for a light emitting diode. Background Art
[0002] Light-emitting diodes (LEDs) are known as green energy sources, with the advantages of energy saving, environmental protection, small size, light weight, long life and low power consumption. In particular, its monochromaticity, dexterity, shock resistance, easy maintenance and digitization make it widely used in modern society. At present, one of the methods to realize white light LED is RGB three-primary color LED mixing. Its advantages are good color rendering and high photoelectric conversion efficiency, and its disadvantages are that the control circuit involved is relatively complex and the cost is high.
[0003] The design of the transition layer of the superlattice is mentioned in 201510891044.2. In addition, the scheme of application 2017111444300 mentions the setting of a color mixing structure of two different lights, such as yellow-green light. The problem with the former is that the electron migration is still insufficient, and the problem with the latter is that it cannot be simply mixed to generate white light. It is necessary to design an epitaxial structure that can realize LED color display. Summary of the invention
[0004] Therefore, it is necessary to provide an epitaxial structure that can realize LED color display and solve the problem of insufficient electron migration in the prior art.
[0005] A mixed-color epitaxial structure comprises a base layer, a buffer layer, a first light-emitting layer, a transition layer of a superlattice structure and a second light-emitting layer grown in sequence; wherein the transition layer comprises a cyclically stacked GaN layer, an InxGa(1-x)N layer and an AlyInzGa(1-yz)N layer, the thickness of the GaN layer gradually increases with the increase of the number of cycles of the cyclic stacking, and the thickness of the InxGa(1-x)N layer and the AlyInzGa(1-yz)N layer gradually decreases with the increase of the number of cycles of the cyclic stacking.
[0006] Specifically, 0≤x≤0.2; 0≤y≤0.1; 0≤z≤0.3.
[0007] Optionally, the first light-emitting layer is a green light-emitting layer, and the second light-emitting layer is a blue light-emitting layer.
[0008] Specifically, the first light emitting layer includes a green light uGaN layer, a green light nGaN layer, a green light MQW quantum well layer, and a green light P layer that are grown in sequence.
[0009] Specifically, the second light emitting layer includes a blue light nGaN layer, a blue light MQW quantum well layer, and a blue light P layer which are grown in sequence.
[0010] Specifically, the blue light has a wavelength of 445nm-475nm, and the green light has a wavelength of 510nm-540nm.
[0011] Furthermore, an ohmic contact layer is grown on the second light-emitting layer.
[0012] Specifically, the number of loop stacking cycles is 3.
[0013] A method for preparing a mixed-color epitaxial structure comprises the following steps: sequentially growing a buffer layer, a first light-emitting layer, a transition layer of a superlattice structure and a second light-emitting layer on a substrate; wherein the transition layer comprises a cyclically stacked GaN layer, an InxGa(1-x)N layer and an AlyInzGa(1-yz)N layer, the thickness of the GaN layer gradually increases as the number of cycles of the cyclic stacking increases, and the thickness of the InxGa(1-x)N layer and the AlyInzGa(1-yz)N layer gradually decreases as the number of cycles of the cyclic stacking increases.
[0014] Specifically, 0≤x≤0.2; 0≤y≤0.1; 0≤z≤0.3.
[0015] Preferably, the first light-emitting layer is a green light-emitting layer, and the second light-emitting layer is a blue light-emitting layer;
[0016] The method also includes the steps of sequentially growing a green light uGaN layer, a green light nGaN layer, a green light MQW quantum well layer, and a green light P layer on the buffer layer; and sequentially growing a blue light nGaN layer, a blue light MQW quantum well layer, and a blue light P layer on the transition layer of the superlattice structure.
[0017] Different from the prior art, the above technical solution enhances electron mobility by setting the thickness of the cyclically stacked InxGa(1-x)N layer and AlyInzGa(1-yz)N layer in the superlattice layer, thereby ultimately achieving the technical effect of enhancing current. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is a schematic diagram of the epitaxial structure of the mixed color described in the specific implementation method,
[0019] Figure 2 Schematic diagram of the transition layer of the superlattice described in a specific implementation manner.
[0020] Description of Reference Numerals
[0021] 100. Grassroots;
[0022] 102. Buffer layer;
[0023] 104. a first light-emitting layer;
[0024] 1041, green light uGaN layer;
[0025] 1042, green light nGaN layer;
[0026] 1043, green light MQW quantum well layer;
[0027] 1044, green light P layer;
[0028] 106. Transition layer;
[0029] 108. a second light-emitting layer;
[0030] 1081, blue light nGaN layer;
[0031] 1082, blue light MQW quantum well layer;
[0032] 1083. Blue light P layer. DETAILED DESCRIPTION
[0033] In order to explain the technical content, structural features, achieved objectives and effects of the technical solution in detail, the following is a detailed description in conjunction with specific embodiments and accompanying drawings.
[0034] See also Figure 1 , a mixed color epitaxial structure, including a base layer 100 (substrate, the substrate material can be sapphire (Al2O3), Si and SiC, etc.), a buffer layer 102, a first light-emitting layer 104, a transition layer 106 of a superlattice structure and a second light-emitting layer 108 grown in sequence. Figure 2 In the embodiment shown, we can see that the transition layer 106 includes a cyclically stacked GaN layer, an InxGa(1-x)N layer and an AlyInzGa(1-yz)N layer, the thickness of the GaN layer gradually increases as the number of cycles of the cyclic stacking increases, and the thickness of the InxGa(1-x)N layer and the AlyInzGa(1-yz)N layer gradually decreases as the number of cycles of the cyclic stacking increases. By setting the thickness of the GaN layer to gradually increase as the number of cycles of the cyclic stacking increases, the thickness of the InxGa(1-x)N layer and the AlyInzGa(1-yz)N layer gradually decreases as the number of cycles of the cyclic stacking increases. In some other specific embodiments, 0≤x≤0.2; 0≤y≤0.1; 0≤z≤0.3 can also be set. Thereby, a gradual thickness gradient can be formed, which can reduce the dislocation density, facilitate current expansion, increase the carrier concentration, and improve the electron mobility.
[0035] The first light-emitting layer and the second light-emitting layer can be arranged as required to obtain the required mixed color light. Figure 1In the specific embodiment shown, the first light-emitting layer 104 is a green light-emitting layer, and the green light has a wavelength of 510nm-540nm. The first light-emitting layer includes a green light uGaN layer 1041, a green light nGaN layer 1042, a green light MQW quantum well layer 1043, and a green light P layer 1044 grown in sequence. The second light-emitting layer 108 is a blue light-emitting layer, and the blue light here has a wavelength of 445nm-475nm. The second light-emitting layer 108 includes a blue light nGaN layer 1081, a blue light MQW quantum well layer 1082, and a blue light P layer 1083 grown in sequence. Of course, the second light-emitting layer can also be set as a green light-emitting layer, and the first light-emitting layer can be set as a blue light-emitting layer; due to the high intensity of blue light, placing the blue light emitting area at the bottom may affect the effect of green light emission. This allows blue light and green light to mix to generate an LED that emits cyan light. The cyan LED after the above mixing scheme can be easily mixed with the red LED to produce white light. Such an LED can replace the three-primary color mixing method and can effectively simplify the control circuit, thereby reducing the cost by about 20% to 50%.
[0036] exist Figure 1 In the further embodiment shown, an ohmic contact layer 110 is also grown on the second light emitting layer 108. By designing the ohmic contact layer, the light-mixing epitaxial structure can emit light.
[0037] like Figure 2 As shown in the figure, the number of cycles of the cyclic stacking is 3, namely, N1 pair, N2 pair, and N3 pair. In the three-layer cyclic stacking, in order to reduce the stress effect, the first cycle matches well with the lattice below, the third cycle matches well with the lattice above, and the second cycle serves to connect the first cycle and the third cycle. On the other hand, it can form a relatively good ohmic contact, so that the product of this solution is not easy to have too high voltage.
[0038] We also provide a method for preparing a mixed-color epitaxial structure, comprising the following steps, sequentially growing a buffer layer, a first light-emitting layer, a transition layer of a superlattice structure, and a second light-emitting layer on a substrate; wherein the transition layer comprises a cyclically stacked GaN layer, an InxGa(1-x)N layer, and an AlyInzGa(1-yz)N layer, the thickness of the GaN layer gradually increases with the increase in the number of cycles of the cyclic stacking, and the thickness of the InxGa(1-x)N layer and the AlyInzGa(1-yz)N layer gradually decreases with the increase in the number of cycles of the cyclic stacking. Wherein, 0≤x≤0.2; 0≤y≤0.1; 0≤z≤0.3. Through the above-mentioned manufacturing method, a gradual thickness gradient can be formed, thereby reducing the dislocation density, facilitating current expansion, increasing the carrier concentration, and improving the electron mobility.
[0039] Preferably, the first light-emitting layer is a green light-emitting layer, and the second light-emitting layer is a blue light-emitting layer;
[0040] The method also includes the steps of sequentially growing a green light uGaN layer, a green light nGaN layer, a green light MQW quantum well layer, and a green light P layer on the buffer layer; and sequentially growing a blue light nGaN layer, a blue light MQW quantum well layer, and a blue light P layer on the transition layer of the superlattice structure. By making a blue-green mixed light epitaxial structure through this step, blue light and green light can be mixed to generate a cyan light emitting LED, and the cyan light LED after the above mixing scheme can be conveniently mixed with a red light LED to generate white light. Such an LED can replace the three-primary color mixing method, and can effectively simplify the control circuit, thereby reducing the cost by about 20% to 50%.
[0041] It should be noted that, although the above embodiments have been described in this article, the scope of patent protection of the present invention is not limited thereby. Therefore, based on the innovative concept of the present invention, changes and modifications made to the embodiments described herein, or equivalent structures or equivalent process changes made using the contents of the present specification and drawings, directly or indirectly applying the above technical solutions to other related technical fields are all included in the scope of protection of the patent of the present invention.
Claims
1. A mixed color epitaxial structure, characterized in that: It includes a base layer, a buffer layer, a first light-emitting layer, a transition layer of a superlattice structure and a second light-emitting layer grown in sequence; wherein the transition layer includes a cyclically stacked GaN layer, an InxGa(1-x)N layer and an AlyInzGa(1-yz)N layer, the thickness of the GaN layer gradually increases with the increase of the number of cycles of the cyclic stacking, and the thickness of the InxGa(1-x)N layer and the AlyInzGa(1-yz)N layer gradually decreases with the increase of the number of cycles of the cyclic stacking.
2. The color-mixing epitaxial structure according to claim 1, characterized in that: 0≤x≤0.2; 0≤y≤0.1; 0≤z≤0.
3.
3. The color-mixing epitaxial structure according to claim 1, characterized in that: The first light-emitting layer is a green light-emitting layer, and the second light-emitting layer is a blue light-emitting layer.
4. The mixed color epitaxial structure according to claim 3, characterized in that: The first light emitting layer includes a green light uGaN layer, a green light nGaN layer, a green light MQW quantum well layer, and a green light P layer grown in sequence, and the second light emitting layer includes a blue light nGaN layer, a blue light MQW quantum well layer, and a blue light P layer grown in sequence.
5. The mixed color epitaxial structure according to claim 3, characterized in that: The blue light has a wavelength of 445nm-475nm, and the green light has a wavelength of 510nm-540nm.
6. The mixed color epitaxial structure according to claim 1, characterized in that: An ohmic contact layer is also grown on the second light-emitting layer.
7. The mixed color epitaxial structure according to claim 1, characterized in that: The number of cycle stacking periods is 3.
8. A method for preparing a mixed color epitaxial structure, characterized in that: The invention comprises the following steps: sequentially growing a buffer layer, a first light-emitting layer, a transition layer of a superlattice structure and a second light-emitting layer on a substrate; wherein the transition layer comprises a cyclically stacked GaN layer, an InxGa(1-x)N layer and an AlyInzGa(1-yz)N layer, the thickness of the GaN layer gradually increases with the increase of the number of cycles of the cyclic stacking, and the thickness of the InxGa(1-x)N layer and the AlyInzGa(1-yz)N layer gradually decreases with the increase of the number of cycles of the cyclic stacking.
9. The method for preparing a mixed-color epitaxial structure according to claim 8, characterized in that: 0≤x≤0.2; 0≤y≤0.1; 0≤z≤0.
3.
10. The method for preparing a mixed-color epitaxial structure according to claim 8, characterized in that: The first light-emitting layer is a green light-emitting layer, and the second light-emitting layer is a blue light-emitting layer; The method also includes the steps of sequentially growing a green light uGaN layer, a green light nGaN layer, a green light MQW quantum well layer, and a green light P layer on the buffer layer; and sequentially growing a blue light nGaN layer, a blue light MQW quantum well layer, and a blue light P layer on the transition layer of the superlattice structure.