Semiconductor device and method for forming the same

By forming a multi-layer stress layer in the trench of the dummy gate structure during the formation of the semiconductor device, the problem of unstable performance of the fin field effect transistor is solved, and the stability and electrical performance of the semiconductor device are improved.

CN111816563BActive Publication Date: 2024-11-19SEMICON MFG INT (SHANGHAI) CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN201910295434.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-04-12
Publication Date
2024-11-19
Estimated Expiration
2039-04-12

AI Technical Summary

Technical Problem

After the size reduction and density of existing semiconductor devices increases, the performance of fin field effect transistors is unstable, resulting in a decrease in leakage current and electrical performance.

Method used

During the formation of a semiconductor device, the first and second trenches are formed on both sides of the dummy gate structure of the dense and sparse regions of the device, and a multi-layer stress layer is formed therein, and the volume of the stress layer is increased by epitaxial growth method. , reduce contact resistance and improve device stability.

Benefits of technology

By increasing the volume of the stress layer in the sparse area of ​​the device, increasing the contact area between the contact holes and the source and drain, balancing the contact resistance of the dense and sparse areas of the device, improving the performance stability and service life of the semiconductor device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111816563B_ABST
    Figure CN111816563B_ABST
Patent Text Reader

Abstract

The present invention provides a semiconductor device and a method for forming the same, comprising the following steps: providing a substrate, the substrate comprising a device dense region and a device sparse region, and a fin portion being formed on the substrate; forming a pseudo gate structure on the substrate, the pseudo gate structure spanning the fin portion; forming a first groove in the fin portion on both sides of the pseudo gate structure in the device dense region, and forming a second groove in the fin portion on both sides of the pseudo gate structure in the device sparse region; forming a first stress layer in the first groove and the second groove; forming a sacrificial sidewall on the sidewall of the pseudo gate structure; forming a second stress layer on the first stress layer of the second groove; removing the sacrificial sidewall; and balancing the contact resistance between the device sparse region and the device dense region by performing secondary epitaxial growth of the stress layer in the device sparse region, thereby improving the stability of the performance of the semiconductor device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor manufacturing, and in particular to a semiconductor device and a method for forming the same. Background Art

[0002] With the rapid development of semiconductor manufacturing technology, semiconductor devices are developing towards higher component density and higher integration. As the most basic semiconductor device, the device is currently being widely used. The control ability of traditional planar devices on channel current has weakened, resulting in short channel effect and leakage current, which ultimately affects the electrical performance of semiconductor devices.

[0003] In order to overcome the short channel effect of the device and suppress leakage current, the prior art proposes a fin field effect transistor (Fin FET). The fin field effect transistor is a common multi-gate device. The structure of the fin field effect transistor includes: a fin and an isolation structure located on the surface of a semiconductor substrate, the isolation structure covers a portion of the sidewall of the fin, a gate structure located on and across the substrate; and a source region and a drain region in the fin located on both sides of the gate structure.

[0004] However, as the size of semiconductor devices decreases and the density of devices increases, the performance of the resulting fin field effect transistors becomes unstable. Summary of the invention

[0005] The problem solved by the present invention is to provide a semiconductor device and a method for forming the same, so that the performance of the formed semiconductor device is stable.

[0006] To solve the above problems, the present invention provides a method for forming a semiconductor device, comprising the steps of: providing a substrate, the substrate comprising a device dense area and a device sparse area, and a fin is formed on the substrate; forming a dummy gate structure on the substrate, the dummy gate structure spanning the fin; forming a first groove in the fin on both sides of the dummy gate structure in the device dense area, and forming a second groove in the fin on both sides of the dummy gate structure in the device sparse area; forming a first stress layer in the first groove and the second groove; forming a sacrificial sidewall on the sidewall of the dummy gate structure; forming a second stress layer on the first stress layer of the second groove; and removing the sacrificial sidewall.

[0007] Optionally, in the device densely populated area, the sacrificial sidewall covers the first stress layer in the first trench.

[0008] Optionally, the material of the sacrificial sidewall includes one or more of silicon nitride, silicon oxide, silicon carbide, silicon carbonitride, organic matter or metal.

[0009] Optionally, the second stress layer is formed by an epitaxial growth method. In the epitaxial growth method for forming the second stress layer, the process temperature is 500-800° C., the reaction chamber pressure is 1-100 Torr, and the reaction gas is silane.

[0010] A semiconductor device formed by the above method includes: a substrate, the substrate including a device dense area and a device sparse area; a fin located on the substrate; a dummy gate structure located on the substrate and spanning the fin; a first trench located in the fin on both sides of the dummy gate structure in the device dense area; a second trench located in the fin on both sides of the dummy gate structure in the device sparse area; a first stress layer located in the first trench and the second trench; and a second stress layer located on the first stress layer in the second trench.

[0011] The present invention also provides another method for forming a semiconductor device, comprising the steps of: providing a substrate, the substrate comprising a device dense area and a device sparse area, and a fin is formed on the substrate; forming a dummy gate structure on the substrate, the dummy gate structure spanning the fin; forming a first groove in the fin on both sides of the dummy gate structure in the device dense area, and forming a second groove in the fin on both sides of the dummy gate structure in the device sparse area; forming a sacrificial sidewall on the sidewall of the dummy gate structure in the device dense area; forming a second stress layer in the second groove; removing the sacrificial sidewall; forming a first stress layer in the first groove and on the second stress layer.

[0012] Optionally, in the device densely populated area, the sacrificial sidewall covers the first trench.

[0013] Optionally, the semiconductor device is a POMS device, and the method used to form the second stress layer is an epitaxial growth method. In the epitaxial growth method for forming the second stress layer, the process temperature is 500-800°C, the reaction chamber pressure is 1-100 Torr, and the reaction gas includes silane and germanium hydrogen gas.

[0014] Optionally, the semiconductor device is a NOMS device, and the method used to form the second stress layer is an epitaxial growth method. In the epitaxial growth method for forming the second stress layer, the process temperature is 500-800°C, the reaction chamber pressure is 1-100 Torr, and the reaction gas includes silane and phosphine gas.

[0015] A semiconductor device formed by the above method includes: a substrate, the substrate including a device dense area and a device sparse area; a fin located on the substrate; a dummy gate structure located on the substrate and spanning the fin; a first trench located in the fin on both sides of the dummy gate structure in the device dense area; a second trench located in the fin on both sides of the dummy gate structure in the device sparse area; a second stress layer located in the second trench; and a first stress layer located in the first trench and on the second stress layer.

[0016] Compared with the prior art, the technical solution of the present invention has the following advantages:

[0017] A stress layer is formed twice in the groove of the device sparse area, which increases the volume of the stress layer formed in the groove of the device sparse area. When a contact hole is subsequently formed, it is convenient to increase the contact area between the contact hole and the source and drain, thereby reducing the contact resistance. At the same time, after the stress layer is formed twice in the groove of the device sparse area, the contact resistance formed in the device sparse area during the subsequent use of the semiconductor device can be balanced with the contact resistance formed in the device dense area, thereby improving the stability of the semiconductor device and reducing the contact resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figures 1 to 4 It is a structural schematic diagram of the process of forming a semiconductor device;

[0019] Figures 5 to 12 is a structural schematic diagram of a semiconductor device forming process in a first embodiment of the present invention;

[0020] Figures 13 to 20 is a schematic structural diagram of a semiconductor device forming process according to a second embodiment of the present invention;

[0021] Figures 21 to 30 is a schematic structural diagram of a semiconductor device forming process according to a third embodiment of the present invention; DETAILED DESCRIPTION

[0022] The performance stability of semiconductor devices currently formed is poor.

[0023] Figures 1 to 4 It is a structural schematic diagram of the process of forming a semiconductor device.

[0024] refer to Figure 1 , providing a substrate 100 including a device dense area 110 , a device sparse area 120 , and a fin 130 .

[0025] refer to Figure 2 , a dummy gate structure 140 is formed on the substrate 100 .

[0026] The dummy gate structure 140 crosses the fin 130 .

[0027] refer to Figure 3 A first trench 111 and a second trench 121 are formed in the fin 130 on both sides of the dummy gate structure 140 .

[0028] refer to Figure 4 A first stress layer 112 and a second stress layer 122 are epitaxially grown in the first trench 111 and the second trench 121 , respectively.

[0029] The inventor has found that when the first stress layer 112 is epitaxially grown in the first trench 111, the growth rate of the first stress layer 112 is fast, and the volume of the formed first stress layer 112 is large. This is because the first stress layer 112 grows simultaneously on the bottom and sidewall of the first trench 111; and when the second stress layer 122 is epitaxially grown in the second trench 121, the volume of the formed second stress layer 122 is small. This is because when the second stress layer 122 is epitaxially grown in the second trench 121, the second stress layer 122 only grows at the bottom of the second trench 121, the growth rate is slow, and the volume of the formed second stress layer 122 is small. The growth rates of the first stress layer 112 and the second stress layer 122 are not balanced, resulting in that when the contact hole is subsequently formed, the contact resistance formed in the device dense area 110 is small, and the contact resistance formed in the device sparse area 120 is large, resulting in that the contact resistance of the device sparse area and the device dense area cannot be balanced, which is easy to cause instability in the performance of the semiconductor device during use.

[0030] The inventors have found that by growing the stress layer twice in the grooves in the sparse area of ​​the device, the volume of the stress layer in the sparse area of ​​the device can be increased. When the contact hole is subsequently formed, the contact area between the contact hole and the source and drain can be increased due to the increase in the volume of the stress layer formed in the sparse area of ​​the device. The larger the contact area, the smaller the contact resistance formed in the sparse area of ​​the device, which can achieve a balance with the contact resistance in the dense area of ​​the device, thereby improving the stability of the performance of the semiconductor device.

[0031] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0032] First embodiment

[0033] Figures 5 to 12 It is a structural schematic diagram of the semiconductor device forming process in the first embodiment of the present invention.

[0034] First reference Figure 5, providing a substrate 200 , wherein the substrate 200 includes a device dense area 210 and a device sparse area 220 .

[0035] In this embodiment, the material of the substrate 200 is single crystal silicon; in other embodiments, the substrate 200 can be single crystal silicon, polycrystalline silicon or amorphous silicon; the substrate 200 can also be a semiconductor material such as silicon, germanium, silicon germanium, gallium arsenide, etc.

[0036] refer to Figure 6 , a fin 300 is formed on the substrate 200 .

[0037] The method for forming the fin 300 includes: first forming a photoresist layer on the substrate 200; after exposure and development processes, forming a photoresist pattern in the photoresist layer; and then etching the substrate 200 using the patterned photoresist layer as a mask, thereby forming the fin 300 on the substrate 200.

[0038] refer to Figure 7 , a dummy gate structure 400 is formed on the substrate 200 , and the dummy gate structure 400 crosses the fin 300 .

[0039] In this embodiment, the material of the dummy gate structure 400 is polysilicon; in other embodiments, the material of the dummy gate structure 400 may also be amorphous carbon or silicon nitride.

[0040] The method for forming the pseudo gate structure 400 includes: forming a gate oxide layer (not shown in the figure) on the surface of the substrate 200, forming a gate layer on the gate oxide layer, and forming a patterned layer on the gate layer, wherein the patterned layer covers the corresponding area where the pseudo gate structure 400 needs to be formed; using the patterned layer as a mask, etching the gate layer and the gate oxide layer until the substrate 200.

[0041] The material of the gate oxide layer is silicon oxide; the gate oxide layer can be formed by a thermal oxidation process, an atomic deposition process or a chemical vapor deposition process.

[0042] In this embodiment, the gate layer needs to be removed later and replaced with a gate dielectric layer of a high-K dielectric material and a gate layer of a metal material.

[0043] refer to Figure 8 , a first trench 211 is formed in the fin 300 on both sides of the dummy gate structure 400 in the device dense area 210 , and a second trench 221 is formed in the fin 300 on both sides of the dummy gate structure 400 in the device sparse area 220 .

[0044] In this embodiment, the method for forming the first groove 211 and the second groove 221 is dry etching; the parameters of the dry etching include: the etching gases used include HBr and Ar, wherein the flow rate of HBr is 10sccm~1000sccm, and the flow rate of Ar is 10sccm~1000sccm.

[0045] In other embodiments, the method for forming the first trench 211 and the second trench 221 is anisotropic wet etching or the like, and a suitable etching method can be selected according to actual needs.

[0046] refer to Fig. 9 , a first stress layer 230 is formed in the first trench 211 and the second trench 221 .

[0047] In this embodiment, the first stress layer 230 is formed by an epitaxial growth method; in other embodiments, the method of forming the first stress layer 230 is not limited to the epitaxial growth method.

[0048] In this embodiment, when the semiconductor device is a POMS device, the process conditions for forming the first stress layer 230 are to control the temperature within the range of 500 to 800°C and the pressure within the range of 1 to 100 Torr, the selected gas includes a mixed gas of silane (SiH4) and germanium hydrogen gas (GeH4), the gas flow rate is controlled within the range of 70 to 300 sccm and the time is controlled within the range of 3 to 120 s.

[0049] In this embodiment, when the semiconductor device is a NOMS device, the process conditions for forming the first stress layer 230 are to control the temperature within the range of 500 to 800°C and the pressure within the range of 1 to 100 Torr. The selected gas includes a mixture of silane (SiH4) and phosphine gas (PH3). The gas flow rate is controlled within the range of 70 to 300 sccm and the time is controlled within the range of 3 to 120 s.

[0050] refer to Fig.10 , a sacrificial spacer 500 is formed on the sidewall of the dummy gate structure 400 .

[0051] In this embodiment, the sacrificial spacer 500 covers the first stress layer 230 in the first trench 211 .

[0052] In the present embodiment, the thickness of the sacrificial sidewall 500 in the device dense area is between 15 and 30 nanometers; when the thickness of the sacrificial sidewall 500 is less than 15 nanometers, the sacrificial sidewall 500 adjacent to the sidewall of the pseudo gate structure 400 cannot completely cover the first stress layer 230 formed in the first groove 211, resulting in the subsequent epitaxial growth, and the stress layer will be formed again in the first groove 211, increasing the volume of the first stress layer 230; when the thickness of the sacrificial sidewall 500 is greater than 30 nanometers, the formed sacrificial sidewall 500 is too thick, resulting in a waste of resources.

[0053] In this embodiment, the thickness of the sacrificial spacer 500 formed in the device dense area 210 and the device sparse area 220 is different; in other embodiments, the thickness of the sacrificial spacer 500 in the device dense area 210 and the device sparse area 220 may be the same.

[0054] In this embodiment, the material of the sacrificial sidewall 500 is silicon nitride; in other embodiments, the material of the sacrificial sidewall 500 may also be one or more of silicon oxide, silicon carbide, silicon carbonitride, organic matter or metal.

[0055] In this embodiment, the purpose of the sacrificial sidewall 500 is to cover the first stress layer 230 formed in the first trench 211 in order to prevent the stress layer from growing again in the first trench 211 when epitaxial growth is performed again in the subsequent process.

[0056] refer to Fig.11 , forming a second stress layer 240 on the first stress layer 230 in the second trench 221 .

[0057] In this embodiment, the second stress layer 240 is formed by epitaxial growth, and the reaction gas includes silane (SiH4) or a combination of silane (SiH4) and germanium hydrogen gas (GeH4) or a combination of silane (SiH4) and phosphine gas (PH3).

[0058] In this embodiment, the method used to form the second stress layer 240 is an epitaxial growth method. In the epitaxial growth method for forming the second stress layer 240, the process temperature is 500-800°C, the reaction chamber pressure is 1-100 Torr, the reaction gas is silane (SiH4), and the reaction time is controlled at 3-120s.

[0059] In the present embodiment, the reaction gas for forming the second stress layer 240 is silane (SiH4), the purpose of which is to simplify the process and improve production efficiency. The use of silane (SiH4) can form the second stress layer 240 without applying stress, and is suitable for forming the second stress layer 240 in both the device sparse area of ​​the POMS device and the device sparse area of ​​the NOMS device, so that the production process can be simplified and the production efficiency can be improved. At the same time, the use of silane (SiH4) will not affect the pressure of the epitaxial growth of the POMS device or the NOMS device.

[0060] In the present embodiment, the purpose of forming the second stress layer 240 on the first stress layer 230 of the second groove 221 is to increase the volume of the stress layer in the second groove 221 in the device sparse area 220, so as to increase the contact area between the contact hole and the source and drain when the contact hole is subsequently formed, thereby reducing the contact resistance in the device sparse area 220, thereby achieving a balance with the contact resistance in the device dense area. In this way, during the use of the semiconductor device, the stability of the use of the semiconductor device will not be affected due to the large difference in contact resistance between the device sparse area and the device dense area.

[0061] refer to Fig.12 , remove the sacrificial sidewall 500.

[0062] In this embodiment, the sacrificial sidewall 500 may be removed by ashing. In other embodiments, the sacrificial sidewall 500 may be removed by wet etching or other processes.

[0063] A semiconductor device formed by the above method comprises a substrate 200, wherein the substrate 200 comprises a device dense region 210 and a device sparse region 220; a fin 300 located on the substrate 200; a dummy gate structure 400 located on the substrate 200 and spanning the fin 300; a first groove 211 located in the fin 300 on both sides of the dummy gate structure 400 in the device dense region 210; a second groove 221 located in the fin 300 on both sides of the dummy gate structure 400 in the device sparse region 220; a first stress layer 230 located in the first groove 211 and the second groove 221; and a second stress layer 240 located on the first stress layer 230 in the second groove 221.

[0064] Second embodiment

[0065] Figures 13 to 20 It is a structural schematic diagram of the semiconductor device forming process in the second embodiment of the present invention.

[0066] refer to Fig.13, providing a substrate 200 , wherein the substrate 200 includes a device dense area 210 and a device sparse area 220 .

[0067] refer to Fig.14 , a fin 300 is formed on the substrate 200 .

[0068] In this embodiment, the steps of forming the fin 300 are the same as the method in the first embodiment; in other embodiments, different methods may be used to form the fin 300.

[0069] refer to Fig.15 , a dummy gate structure 400 is formed on the substrate 200 , and the dummy gate structure 400 crosses the fin 300 .

[0070] In this embodiment, the method for forming the dummy gate structure 400 is the same as the method in the first embodiment; in other embodiments, other methods may be used to form the dummy gate structure 400.

[0071] refer to Fig.16 , a first trench 211 is formed in the fin 300 on both sides of the dummy gate structure 400 in the device dense area 210 , and a second trench 221 is formed in the fin 300 on both sides of the dummy gate structure 400 in the device sparse area 220 .

[0072] In this embodiment, the fin 300 is wet etched, and the parameters of the wet etching process include: an aqueous solution of HNO3 and HF, wherein the volume ratio of HNO3, HF and H2O is 1:3:(10~~800), and the temperature is 40℃~90℃.

[0073] In other embodiments, the method for etching the fin 300 can be set according to actual process requirements.

[0074] refer to Fig.17 , a sacrificial spacer 500 is formed on the sidewall of the dummy gate structure 400 in the device dense area 210 .

[0075] In this embodiment, the sacrificial sidewall 500 completely covers and fills the first trench 211 , with the purpose of first covering the first trench 211 so that a stress layer will not be formed in the first trench 211 in the subsequent epitaxial growth process.

[0076] In this embodiment, the material of the sacrificial sidewall 500 is silicon carbonitride; in other embodiments, the material of the sacrificial sidewall 500 may also be one or more of silicon oxide, silicon carbide, silicon nitride, organic matter or metal.

[0077] refer to Fig.18 , a second stress layer 240 is formed in the second trench 221 .

[0078] In this embodiment, the second stress layer 240 is formed by epitaxial growth, and the reaction gas includes silane (SiH4) or a combination of silane (SiH4) and germanium hydrogen gas (GeH4) or a combination of silane (SiH4) and phosphine gas (PH3).

[0079] In this embodiment, the process temperature, reaction chamber pressure and reaction time for forming the second stress layer 240 are the same as those in the first embodiment; in other embodiments, different process conditions may also be used.

[0080] refer to Fig.19 , remove the sacrificial sidewall 500.

[0081] In this embodiment, chemical reagents are used to remove the sacrificial sidewalls 500 .

[0082] refer to Fig. 20 , a first stress layer 230 is formed in the first trench 211 ; and a first stress layer 230 is formed on the second stress layer 240 .

[0083] In this embodiment, the process conditions for forming the first stress layer 230 are the same as those in the first embodiment; in other embodiments, different process conditions may be used to form the first stress layer 230 .

[0084] A semiconductor device formed by the above method comprises a substrate 200, wherein the substrate 200 comprises a device dense region 210 and a device sparse region 220; a fin 300 located on the substrate 200; a dummy gate structure 400 located on the substrate 200 and spanning the fin 300; a first groove 211 located in the fin 300 on both sides of the dummy gate structure 400 in the device dense region 210; a second groove 221 located in the fin 300 on both sides of the dummy gate structure 400 in the device sparse region 220; a second stress layer 240 located in the second groove 221; and a first stress layer 230 located in the first groove 211 and on the second stress layer 240.

[0085] Third embodiment

[0086] Figures 21 to 30 It is a structural schematic diagram of the semiconductor device forming process in the third embodiment of the present invention.

[0087] In this embodiment, the device is a POMS device.

[0088] refer to Fig.21 , providing a substrate 200 , wherein the substrate 200 includes a device dense area 210 and a device sparse area 220 .

[0089] refer to Fig. 22 , a fin 300 and an isolation structure 600 are formed on the substrate 200 .

[0090] In this embodiment, an isolation structure 600 is formed on the substrate 200 ; in other embodiments, the isolation structure 600 may not be formed on the substrate 200 .

[0091] In this embodiment, the isolation structure 600 may be a shallow trench isolation structure, but is not limited to the shallow trench isolation structure. The isolation structure 600 is used to achieve mutual isolation between devices.

[0092] The steps of forming the isolation structure 600 include etching the substrate 200 to form an isolation trench (not shown) in the semiconductor substrate 200 ; filling the isolation trench with isolation material, and planarizing the isolation material to form the isolation structure 600 .

[0093] The isolation material may be silicon oxide, and the process of filling the isolation trench with silicon oxide may be chemical vapor deposition or physical vapor deposition.

[0094] refer to Fig.23 , a dummy gate structure 400 is formed on the substrate 200 , and the dummy gate structure 400 crosses the fin 300 .

[0095] In this embodiment, the method of forming the dummy gate structure 400 is the same as that of the first embodiment.

[0096] refer to Fig.24 , a mask layer 401 is formed on the dummy gate structure 400 .

[0097] In this embodiment, a mask layer 401 is further formed on the dummy gate structure 400 ; in other embodiments, the mask layer 401 may not be formed on the dummy gate structure 400 .

[0098] In this embodiment, the material of the mask layer 401 is silicon carbide; in other embodiments, the mask layer 301 may also be made of silicon oxide or silicon nitride.

[0099] refer to Fig.25 , forming a sidewall spacer 402 on the sidewall of the dummy gate structure 400 .

[0100] In this embodiment, after forming the dummy gate structure 400 , a sidewall spacer 402 is further formed on the sidewall of the dummy gate structure 400 . In other embodiments, the sidewall spacer 402 may not be formed on the sidewall of the dummy gate structure 400 .

[0101] The sidewall spacer 402 is used to define the position of the subsequently formed source and drain doping layer, and the sidewall spacer 302 is used to protect the sidewall of the dummy gate structure 400 to prevent the subsequently formed gate layer from having morphological defects that affect the electrical performance of the semiconductor structure.

[0102] In this embodiment, the material of the sidewall 402 is silicon oxide; in other embodiments, the material of the sidewall 402 may also be one or more of silicon nitride, silicon oxynitride, silicon oxycarbide, silicon carbonitride or silicon carbon oxynitride.

[0103] refer to Fig.26 , a first trench 211 is formed in the fin 300 on both sides of the dummy gate structure 400 in the device dense area 210 , and a second trench 221 is formed in the fin 300 on both sides of the dummy gate structure 400 in the device sparse area 220 .

[0104] refer to Fig. 27 , a sacrificial spacer 500 is formed on the sidewall of the spacer 402 in the device dense area 210 .

[0105] In this embodiment, the sacrificial spacer 500 covers the first trench 211 .

[0106] refer to Fig.28 , a second stress layer 240 is formed in the second trench 221 .

[0107] In this embodiment, the method used to form the second stress layer 240 is epitaxial growth method, and the reaction gas is a combination of silane (SiH4) and germanium hydrogen gas (GeH4); wherein the reaction temperature is controlled between 500 and 800°C, the chamber pressure is controlled between 1 and 100 Torr, and the reaction time is controlled between 3 and 120s.

[0108] In the present embodiment, the purpose of performing the first epitaxial growth in the second groove 221 in the device sparse area 220 is to increase the volume of the stress layer in the second groove 221, so that during the subsequent second epitaxial growth, the volume of the stress layer epitaxially grown in the second groove 221 can be balanced with the volume of the stress layer in the first groove 211, and when forming the contact hole, the contact resistance of the device sparse area 220 can be balanced with the contact resistance of the device dense area 210, thereby improving the stability of the performance of the semiconductor device.

[0109] refer to Fig.29 , remove the sacrificial sidewall 500.

[0110] In this embodiment, the sacrificial sidewall spacer 500 is removed by ashing.

[0111] refer to Fig.30, a first stress layer 230 is formed in the first trench 211 ; and a first stress layer 230 is formed on the second stress layer 240 .

[0112] In the present embodiment, the first stress layer 230 located on the second stress layer 240 is formed by performing secondary epitaxial growth in the device sparse area 220, so that the volume of the stress layer grown in the second groove 221 is balanced with the volume of the stress layer grown in the first groove 211, thereby balancing the contact resistance formed in the device sparse area 220 and in the device dense area 210, thereby improving the stability of the performance of the semiconductor device.

[0113] A semiconductor device formed by the above method comprises a substrate 200, wherein the substrate 200 comprises a device dense area 210 and a device sparse area 220; a fin 300 located on the substrate 200; an isolation structure 600 located on the substrate 200; a dummy gate structure 400 located on the substrate 200 and spanning the fin 300; a mask layer 401 located on the top of the dummy gate structure 400; a sidewall 402 located on the sidewall of the dummy gate structure 400; a first trench 211 located in the fin 300 on both sides of the sidewall 402 of the device dense area 210; a second trench 221 located in the fin 300 on both sides of the dummy gate structure 400 of the device sparse area 220; a second stress layer 240 located in the second trench 221; and a first stress layer 230 located in the first trench 211 and on the second stress layer 240.

[0114] Fourth embodiment

[0115] The fourth embodiment differs from the third embodiment only in that the method of forming the second stress layer 240 is different.

[0116] In this embodiment, the device is a NOMS device.

[0117] In this embodiment, the method used to form the second stress layer is an epitaxial growth method. In the epitaxial growth method for forming the second stress layer, the process temperature is 50 to 800°C, the reaction chamber pressure is 1 to 100 Torr, the reaction gas includes silane (SiH4) and phosphine gas (PH3), and the reaction time is 3 to 120s.

[0118] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for forming a semiconductor device, characterized in that: include: Providing a substrate, the substrate comprising a device-intensive region and a device-sparse region, and a fin portion is formed on the substrate; forming a dummy gate structure on the substrate, wherein the dummy gate structure spans across the fin; Forming a first trench in the fins on both sides of the dummy gate structure in the device dense area, and forming a second trench in the fins on both sides of the dummy gate structure in the device sparse area; forming a first stress layer in the first trench and the second trench; forming a sacrificial sidewall spacer on the sidewall of the dummy gate structure, wherein the sacrificial sidewall spacer covers the first stress layer in the first trench; forming a second stress layer on the first stress layer in the second trench; The sacrificial sidewall is removed.

2. The method for forming a semiconductor device according to claim 1, wherein: In the device-intensive area, the sacrificial spacer covers the first stress layer in the first trench.

3. The method for forming a semiconductor device according to claim 2, wherein: The material of the sacrificial sidewall spacer includes one or more of silicon nitride, silicon oxide, silicon carbide, and silicon carbonitride.

4. The method for forming a semiconductor device according to claim 1, wherein: The method used to form the second stress layer is an epitaxial growth method. In the epitaxial growth method for forming the second stress layer, the process temperature is 500-800° C., the reaction chamber pressure is 1-100 Torr, and the reaction gas is silane.

5. A semiconductor device formed by the method according to any one of claims 1 to 4, characterized in that: include: A substrate, wherein the substrate includes a device-intensive region and a device-sparse region; A fin portion, located on the substrate; a dummy gate structure, located on the substrate and spanning the fin; A first trench is located in the fins on both sides of the dummy gate structure in the device dense area; A second trench is located in the fins on both sides of the dummy gate structure in the device sparse area; A first stress layer, located in the first trench and the second trench; The second stress layer is located on the first stress layer in the second groove.

6. A method for forming a semiconductor device, characterized in that: include, Providing a substrate, the substrate comprising a device-intensive region and a device-sparse region, and a fin portion is formed on the substrate; forming a dummy gate structure on the substrate, wherein the dummy gate structure spans across the fin; Forming a first trench in the fins on both sides of the dummy gate structure in the device dense area, and forming a second trench in the fins on both sides of the dummy gate structure in the device sparse area; Forming a sacrificial spacer on the sidewall of the dummy gate structure in the device dense area, wherein the sacrificial spacer fills the first trench; forming a second stress layer in the second trench; removing the sacrificial side wall; A first stress layer is formed in the first trench and on the second stress layer.

7. The method for forming a semiconductor device according to claim 6, wherein: In the device densely populated area, the sacrificial spacer covers the first trench.

8. The method for forming a semiconductor device according to claim 6, wherein: When the semiconductor device is a POMS device, the method used to form the second stress layer is an epitaxial growth method. In the epitaxial growth method for forming the second stress layer, the process temperature is 500-800° C., the reaction chamber pressure is 1-100 Torr, and the reaction gas includes silane and germanium hydrogen gas.

9. The method for forming a semiconductor device according to claim 6, wherein: When the semiconductor device is a NOMS device, the method used to form the second stress layer is an epitaxial growth method. In the epitaxial growth method for forming the second stress layer, the process temperature is 500-800°C, the reaction chamber pressure is 1-100 Torr, and the reaction gas includes silane and phosphine gas.

10. A semiconductor device formed by the method according to any one of claims 6 to 9, characterized in that: include: A substrate, wherein the substrate includes a device-intensive region and a device-sparse region; A fin portion, located on the substrate; a dummy gate structure, located on the substrate and spanning the fin; A first trench is located in the fins on both sides of the dummy gate structure in the device dense area; A second trench is located in the fins on both sides of the dummy gate structure in the device sparse area; A second stress layer, located in the second groove; The first stress layer is located in the first groove and on the second stress layer.

Citation Information

Patent Citations

  • Halbleiterstruktur und verfahren zu deren herstellung

    CN103219340A

  • Semiconductor structure forming method

    CN106373924A

  • Manufacturing method of semiconductor structure

    CN107481933A

  • Germanium silicon source-and-drain electrode and preparing method thereof

    CN107634092A

  • Finfets and method of fabricating the same

    US20130221443A1