Solid electrolyte and battery using the same

By using a first solid electrolyte material with high ion conductivity and a second solid electrolyte material with low Young's modulus in the solid electrolyte, and forming a grain boundary layer therebetween, the defect of the layered structure of the solid electrolyte is solved under high pressure. The problem is that high energy density and stable ion conductivity are achieved.

CN112602222BActive Publication Date: 2024-11-05PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980053293.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-11-16
Filing Date
2019-10-07
Publication Date
2024-11-05
Estimated Expiration
2039-10-07

AI Technical Summary

Technical Problem

Existing solid electrolytes are prone to layered structure defects under high pressure, resulting in a significant reduction in ion conductivity under atmospheric pressure, affecting the energy density of the battery.

Method used

Particles composed of a first solid electrolyte material with high ion conductivity and a second solid electrolyte material with low Young's modulus are used, and a thin grain boundary layer is formed therebetween, and a dense solid electrolyte is formed by a powder pressing process to form a dense solid electrolyte to Inhibit the occurrence of hierarchical structure.

Benefits of technology

The solid electrolyte formed under high pressure has high effective ion conductivity and high energy density, and maintains a high ion conductivity under atmospheric pressure, thereby avoiding the occurrence of structural defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112602222B_ABST
    Figure CN112602222B_ABST
Patent Text Reader

Abstract

The present disclosure provides a solid electrolyte with high ion conductivity, which can realize a secondary battery with high energy density when used in a secondary battery. The solid electrolyte (1000) involved in the present disclosure includes a first particle (101) composed of a first solid electrolyte material and a second particle (102) composed of a second solid electrolyte material. The ion conductivity of the first solid electrolyte material is higher than that of the second solid electrolyte material. The Young's modulus of the second solid electrolyte material is lower than that of the first solid electrolyte material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a solid electrolyte and a battery using the same. Background Art

[0002] Patent Document 1 discloses an all-solid-state battery containing lithium sulfide having an argyrodite crystal structure. Patent Document 2 discloses an all-solid-state battery having a solid electrolyte in which a sulfide-based glass and crystals are mixed.

[0003] Prior Art Literature

[0004] Patent Document 1: U.S. Patent Application Publication No. 2016 / 0293946

[0005] Patent Document 2: Japanese Patent Application Publication No. 2011-154900 Summary of the invention

[0006] Problems to be solved by the invention

[0007] An object of the present disclosure is to provide a solid electrolyte having high ion conductivity.

[0008] Means for solving problems

[0009] The solid electrolyte disclosed herein comprises:

[0010] first particles composed of a first solid electrolyte material; and

[0011] second particles composed of a second solid electrolyte material,

[0012] The first solid electrolyte material has a higher ion conductivity than the second solid electrolyte material, and

[0013] The second solid electrolyte material has a lower Young's modulus than the first solid electrolyte material.

[0014] Effects of the Invention

[0015] The present disclosure provides a solid electrolyte having high ion conductivity. A battery having the solid electrolyte has high energy density. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 A schematic diagram showing a solid electrolyte 1000 in Embodiment 1.

[0017] Figure 2 A cross-sectional view of a battery 2000 according to the second embodiment is shown.

[0018] Figure 3 A cross-sectional view of a battery 3000 according to a modification of the second embodiment is shown. DETAILED DESCRIPTION

[0019] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.

[0020] (Implementation Method 1)

[0021] The solid electrolyte in the first embodiment includes first particles and second particles composed of a first solid electrolyte material and a second solid electrolyte material, respectively. The first solid electrolyte material has a higher ion conductivity than the second solid electrolyte material. The second solid electrolyte material has a lower Young's modulus than the first solid electrolyte material.

[0022] In the first embodiment, a solid electrolyte having high ion conductivity and without structural defects is formed at a high density. The solid electrolyte of the first embodiment has a high effective ion conductivity. A battery having the solid electrolyte of the first embodiment has a high energy density. In this specification, the effective ion conductivity of the solid electrolyte refers to the ion conductivity when the solid electrolyte is actually used. As an example, the effective ion conductivity refers to the ion conductivity of the solid electrolyte contained in the battery.

[0023] Generally, when high pressure is applied to particles of a solid electrolyte having a high Young's modulus and high ionic conductivity, delamination is likely to occur between particles due to stress caused by pressure and density distribution. In contrast, in the solid electrolyte of embodiment 1, the occurrence of delamination is suppressed. Therefore, the solid electrolyte of embodiment 1 has high ionic conductivity (e.g., high effective ionic conductivity). Furthermore, a battery using the solid electrolyte of embodiment 1 has a high energy density.

[0024] Generally, the ion conductivity of a solid electrolyte composed of a powder compact is measured by placing the solid electrolyte in a mold under high pressure. However, batteries with solid electrolytes are usually released from high pressure.

[0025] When a solid electrolyte is released from pressure (e.g., when the solid electrolyte is placed under atmospheric pressure), structural defects such as delamination are generated in the solid electrolyte due to uneven pressure distribution and rebound stress. As a result, it is noted that the ion conductivity of the solid electrolyte measured under high pressure is significantly different from that of the solid electrolyte measured under atmospheric pressure.

[0026] The solid electrolyte of embodiment 1 may further include a grain boundary layer composed of a third solid electrolyte material. In the case where the solid electrolyte of embodiment 1 includes a grain boundary layer, the thickness of the grain boundary layer may be smaller than the particle size of the first particle and the particle size of the second particle. The Young's modulus of the third solid electrolyte material may be less than the Young's modulus of the second solid electrolyte material. The Young's modulus of the third solid electrolyte material may also be lower than the Young's modulus of the second solid electrolyte material. In the case where the solid electrolyte layer of embodiment 1 also contains such a grain boundary layer, the occurrence of delamination is further suppressed.

[0027] Figure 1 A schematic diagram showing a solid electrolyte 1000 in Embodiment 1. Figure 1 The solid electrolyte according to Embodiment 1 will be described.

[0028] The solid electrolyte 1000 includes the first particles 101 , the second particles 102 , and the grain boundary layer 103 . The solid electrolyte 1000 may not include the grain boundary layer 103 .

[0029] The first particle 101 is made of a first solid electrolyte material. The second particle 102 is made of a second solid electrolyte material. The first solid electrolyte material has a higher ion conductivity than the second solid electrolyte material. The second solid electrolyte material has a lower Young's modulus than the first solid electrolyte material.

[0030] The grain boundary layer 103 may exist between the first particle 101 and the second particle 102 .

[0031] The grain boundary layer 103 may exist between two adjacent first particles 101. Similarly, the grain boundary layer 103 may exist between two adjacent second particles 102.

[0032] The grain boundary layer 103 is composed of the third solid electrolyte material.

[0033] The first particles 101 are bonded to each other via the second particles 102 and the grain boundary layer 103. The second particles 102 have a lower Young's modulus than the first particles 101. The grain boundary layer 103 preferably has a lower Young's modulus than the first particles 101. The Young's modulus of the third solid electrolyte material is preferably equal to or less than that of the second solid electrolyte material.

[0034] The presence of the grain boundary layer 103 as described above can suppress the occurrence of structural defects such as delamination even when the particles are densely packed while applying a high pressure to the particles to form the solid electrolyte 1000. As a result, a solid electrolyte having a high effective ion conductivity can be obtained. The mechanism by which the grain boundary layer 103 suppresses the occurrence of structural defects such as delamination will be described in detail later.

[0035] (Method of Manufacturing Solid Electrolyte 1000)

[0036] Hereinafter, an example of a method for producing solid electrolyte 1000 will be described.

[0037] First, the powder of the first particles 101 and the powder of the second particles 102 are mixed to obtain a mixed powder.

[0038] As will be demonstrated in the examples described later, the powder of the second particle 102 may contain a component for forming the grain boundary layer 103. As an example, the powder of the second particle 102 is a glass powder containing lithium sulfide and phosphorus sulfide. The glass powder contains a crystalline component and an amorphous component. The second particle 102 and the grain boundary layer 103 are respectively composed of a crystalline component and an amorphous component.

[0039] Next, the mixed powder is pressed and molded to obtain the solid electrolyte 100. Hereinafter, such a production method is referred to as a "powder pressing process."

[0040] Since the Young's modulus of the second particle 102 is lower than that of the first particle 101, the second particle 102 is more easily deformed than the first particle 101. Therefore, when pressure is applied, the second particle 102 is deformed in a manner that is compatible with the shape of the gap between the first particles 101. As a result, the second particle 102 is filled in the gap. In this way, a dense solid electrolyte 1000 can be obtained.

[0041] Furthermore, by filling the second particles 102 in the spaces between the first particles 101, the spaces in the solid electrolyte layer 1000 are reduced, thereby improving the ion conductivity.

[0042] The term "particle" used in this specification without distinguishing between the first particle 101 and the second particle 102 refers to the first particle 101 and the second particle 102. The gap between two adjacent particles is filled with a grain boundary layer 103. Therefore, the surface of each particle is in contact with the grain boundary layer 103. The grain boundary layer 103 improves the electrical bonding between two adjacent particles. In other words, in the absence of the grain boundary layer 103, a part of the surface of the particle has not only a contact portion that is in direct contact with the surface of the adjacent particle, but also a non-contact portion that is not in contact with the surface of other particles. In the case where the grain boundary layer 103 is filled in the gap, the grain boundary layer 103 is in contact with the non-contact portion. Therefore, the non-contact portion is in indirect contact with the surface of other particles via the grain boundary layer 103. In this way, the grain boundary layer 103 improves the electrical bonding between two adjacent particles. Note that the first particle 101, the second particle 102 and the grain boundary layer 103 are all composed of solid electrolyte materials.

[0043] In this way, a fine structure is formed in the solid electrolyte 1000. In the fine structure, the soft second particles 102 exist between the first particles 101 so that the gaps between the hard first particles 101 having a high Young's modulus are filled with the second particles 102.

[0044] The grain boundary layer 103 may exist between the first particles 101 so that the gaps between the first particles 101 are filled with the grain boundary layer 103. Similarly, the grain boundary layer 103 may exist between the second particles 102 so that the gaps between the second particles 102 are filled with the grain boundary layer 103.

[0045] Fatigue stress is generated by the rebound after pressure release and the unevenness of pressure distribution, and this fatigue stress is absorbed by the soft organizational structure with ion conductivity (that is, the organizational structure composed of the second particles 102 and the grain boundary layer 103). In this way, even in the case of forming the solid electrolyte 1000 by making the particles high-density under high pressure, structural defects such as delamination in the solid electrolyte 1000 can be suppressed. As a result, a solid electrolyte 1000 with high ion conductivity, high density and high effective ion conductivity is formed. In addition, a battery having a solid electrolyte 1000 with such a high effective ion conductivity has a high energy density. Once again, the microstructure does not need to contain the grain boundary layer 103.

[0046] As described above, the first particle 101, the second particle 102, and the grain boundary layer 103 are composed of a solid electrolyte material. The thickness of the grain boundary layer 103 is smaller than the size of the first particle 101 and the size of the second particle 102. As an example, the thickness of the grain boundary layer 103 may be less than one tenth of the particle size of the first particle 101, and may be less than one tenth of the particle size of the second particle 102. The thickness of the grain boundary layer 103 may be, for example, not less than 2 nanometers and not more than 30 nanometers.

[0047] The ion conductivity of the third solid electrolyte material may be lower than that of the first solid electrolyte material and the second solid electrolyte material. As described above, the third solid electrolyte material is very thin, so the third solid electrolyte material does not have a significant effect on the ion conductivity of the solid electrolyte 1000 as a whole.

[0048] Examples of the solid electrolyte material used for the first particles 101, the second particles 102, and the grain boundary layer 103 include well-known solid electrolyte materials used for batteries. Of course, metal ions such as Li ions and Mg ions are conducted in the solid electrolyte material.

[0049] Examples of solid electrolyte materials are sulfides, oxides, and halides.

[0050] Examples of sulfides include Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, Li2S-SiS2-LiI, Li2S-SiS2-Li3PO4, Li2S-Ge2S2, Li2S-GeS2-P2S5 or Li2S-GeS2-ZnS.

[0051] A halide is, for example, a compound composed of Li, M' and X'. M' is at least one element selected from metal elements and metalloid elements other than Li. X' is at least one element selected from F, Cl, Br and I. "Metal elements" refer to all elements contained in Groups 1 to 12 of the periodic table (except hydrogen) and all elements contained in Groups 13 to 16 of the periodic table (except B, Si, Ge, As, Sb, Te, C, N, P, O, S and Se). "Metalloid elements" refer to B, Si, Ge, As, Sb and Te. For example, M' may contain Y (= yttrium). Examples of halides containing Y are Li3YCl6 or Li3YBr6.

[0052] Examples of oxides include Li-Al-(Ge,Ti)-PO-based materials or Li7La3Zr2O 12 Oxides mainly composed of garnet materials.

[0053] In addition, as the solid electrolyte material, a lithium-containing metal oxide, a lithium-containing metal nitride, lithium phosphate (ie, Li 3 PO 4 ), or a lithium-containing transition metal oxide may be used.

[0054] Examples of lithium-containing metal oxides are Li2-SiO2 or Li2-SiO2-P2O5.

[0055] Examples of lithium-containing metal nitrides include Li 2.9 PO 3.3 N 0.46 .

[0056] An example of the lithium-containing transition metal oxide is lithium titanium oxide.

[0057] The solid electrolyte material used for the first particles 101 and the second particles 102 is selected from the above-mentioned solid electrolyte materials so as to have the Young's modulus and ion conductivity as described above.

[0058] The solid electrolyte material used for the grain boundary layer 103 can also be selected from the above-mentioned solid electrolyte materials so as to have the Young's modulus and ion conductivity as described above.

[0059] Solid electrolyte 1000 may contain not only a solid electrolyte material but also a binder. Examples of the binder are polyethylene oxide and polyvinylidene fluoride.

[0060] In order to improve the ion conductivity of the solid electrolyte 1000 , the first solid electrolyte material may include at least one selected from the group consisting of sulfides, oxides, and halides.

[0061] The first solid electrolyte material may include argyrodite-type sulfide in order to improve the ion conductivity of the solid electrolyte 1000. Argentite-type sulfide has intrinsically high ion conductivity.

[0062] Examples of argyrodite-type sulfides include: α PS β Cl γ (wherein 5.5≤α≤6.5, 4.5≤β≤5.5, 0.5≤γ≤1.5).

[0063] Composition formula Li α PS β Cl γ An example of the composition of the argyrodite-type sulfide represented is Li6PS5Cl. Li6PS5Cl has a high ion conductivity in essence in the state of a powder compact. When pressure is applied to Li6PS5Cl in a mold at room temperature (e.g., 25 degrees Celsius), the ion conductivity is, for example, 2 mS / cm or more and 3 mS / cm or less. The Young's modulus of Li6PS5Cl is approximately 0.2 GPa. By including Li6PS5Cl in the first solid electrolyte material, the ion conductivity of the solid electrolyte 1000 can be improved.

[0064] In order to improve the ion conductivity of the solid electrolyte 1000 , the second solid electrolyte material may include at least one selected from the group consisting of sulfides, oxides, and halides.

[0065] The second solid electrolyte material may include LPS-based sulfide in order to improve the ion conductivity of the solid electrolyte 1000. The LPS-based sulfide is a sulfide including lithium sulfide and phosphorus sulfide.

[0066] Examples of lithium sulfides contained in LPS-based sulfides include Li p S (where 1.5≤p≤2.5). Examples of phosphosulfides contained in LPS-based sulfides include P q S5 (where 1.5≤p≤2.5). That is, the LPS sulfide may be Li p SP q S5. In order to improve the ionic conductivity of the solid electrolyte 1000, as an example, Li p SPq S5 can be Li2S-P2S5.

[0067] In order to improve the ion conductivity of the solid electrolyte 1000 , the second solid electrolyte material may include a glassy sulfide having triclinic crystals as a main component.

[0068] The second solid electrolyte material can be a glass electrolyte of LPS-based sulfide with triclinic crystals as the main component. An example of a glass electrolyte is Li2S-P2S5 (Li2S:P2S5=70:30 (molar ratio)). Li2S-P2S5 (Li2S:P2S5=70:30 (molar ratio)) has an ion conductivity of approximately 0.7 mS / cm and a Young's modulus of approximately 0.09 GPa at room temperature (e.g., 25 degrees Celsius) in the state of a pressed powder. When Li6PS5Cl is used as the first solid electrolyte material, Li2S-P2S5 (Li2S:P2S5=70:30 (molar ratio)) can be used as a suitable second solid electrolyte material.

[0069] The grain boundary layer 103 acts as a bonding layer that bonds the particles to each other between the first particles 101 and the second particles 102 adjacent to each other, between the two first particles 101 adjacent to each other, and between the two second particles 102 adjacent to each other. When the solid electrolyte 1000 is formed by a powder pressing process, the Young's modulus of the third solid electrolyte material is less than the Young's modulus of the second particles 102. The particle size of the third solid electrolyte material can be smaller than that of the first particles 101 and the second particles 102.

[0070] The crystallinity of the third solid electrolyte material may be lower than that of the second solid electrolyte material. When the crystallinity of the third solid electrolyte material is lower than that of the second solid electrolyte material, the grain boundary layer 103 functions more effectively as a bonding layer for bonding particles. In this way, even when the particles are densified under high pressure to form the solid electrolyte 1000, the occurrence of structural defects such as delamination can be suppressed. As a result, a solid electrolyte having high effective ion conductivity can be obtained.

[0071] The third solid electrolyte material may be amorphous. When the third solid electrolyte material is amorphous, the grain boundary layer 103 functions more effectively as a bonding layer for bonding particles. In this way, even when the particles are densified under high pressure to form the solid electrolyte 1000, structural defects such as delamination can be suppressed. As a result, a solid electrolyte with high effective ion conductivity can be obtained.

[0072] The third solid electrolyte material may belong to the same material group as the second solid electrolyte material. When the third solid electrolyte material belongs to the same material group as the second solid electrolyte material, a solid electrolyte 1000 having a stable structure can be obtained from the viewpoints of particle bonding and thermal expansion. In addition, since the thermal expansion coefficient of the second particle 102 is substantially equal to the thermal expansion coefficient of the grain boundary layer 103, a solid electrolyte 1000 having high durability against thermal shock and thermal cycles can be obtained.

[0073] Examples of the third solid electrolyte material include (i) amorphous LPS-based glass, or (ii) LPS-based glass having a lower crystallinity and a smaller particle size than the second particles 102 .

[0074] The Young's modulus and ion conductivity of glass electrolytes such as LPS-based glass will change depending on the temperature or history (process) of the heat treatment. Therefore, by adjusting the heat treatment conditions, the crystallinity of the glass electrolyte can be appropriately controlled, so that it can be used as the first to third solid electrolyte materials. The crystallinity of the powder of the solid electrolyte material can be evaluated using the curve graph and half-value width of X-ray diffraction.

[0075] The size of the first particle 101 and the second particle 102 is larger than the thickness of the grain boundary layer 103 (usually less than several tens of nanometers). The average particle size of the first particle 101 and the second particle 102 can be approximately greater than 0.1 micrometer and less than 10 micrometers. The average particle size refers to the value of D50 (cumulative 50% particle size) obtained by evaluating the volume particle size distribution measured by a laser diffraction particle size distribution analyzer.

[0076] The microstructure of solid electrolyte 1000 in Embodiment 1 can be observed using a high-resolution transmission electron microscope (hereinafter referred to as "TEM"). Using TEM, crystals in the microstructure such as lattice images of first particles 101, second particles 102, and grain boundary layers 103 can be observed.

[0077] Generally, in the same or similar chemical composition, as the crystallinity increases, the Young's modulus increases and the ionic conductivity becomes higher.

[0078] The elements of the first particles 101 , the second particles 102 , and the grain boundary layer 103 can be analyzed by energy dispersive X-ray analysis (hereinafter referred to as “EDS”) or electron probe microanalysis (hereinafter referred to as EPMA).

[0079] By using direct probe measurement such as a microprobe system, it is possible to evaluate the particles in the microstructure of solid electrolyte 1000 in Embodiment 1. The ion conductivity on the surface of the particles can also be evaluated in the same manner.

[0080] The hardness (i.e., Young's modulus) of the particles in the solid electrolyte 1000 of the first embodiment is evaluated based on the deformation of the particle shape in the microstructure observed by TEM. For example, the magnitude relationship of the Young's modulus is determined in the order of particles that are not deformed, particles that are deformed due to pressure, and materials that cannot maintain their shape due to pressure and form the grain boundary layer 103. In this way, the relative relationship of the Young's modulus of the particles is determined.

[0081] As described above, the magnitude relationship between the Young's modulus of the first particle 101 and the second particle 102 is determined by microstructural observation using TEM. Similarly, the magnitude relationship between the Young's modulus of the grain boundary layer 103 and the Young's modulus of the first particle 101 and the second particle 102 is also determined by microstructural observation using TEM.

[0082] When it is difficult to determine the magnitude relationship of the Young's modulus by microstructural observation using a TEM, or when it is necessary to obtain the values ​​of the Young's modulus of the particles and the grain boundary layer 103 , the following alternative method can be used.

[0083] In order to measure the actual Young's modulus, a sample without structural defects is required. A portion without structural defects is selected as a sample, or a sample without structural defects is processed to obtain a sample without structural defects, and then the Young's modulus of the sample is measured. As an alternative, for example, a particle with a size of about tens of microns and no structural defects is used as a single sample, and the Young's modulus of the particle is measured.

[0084] The relative relationship can also be compared based on the displacement characteristics corresponding to the pressure when the probe is pressed.

[0085] The relative softness of the particles can be estimated from the ratio of displacement to the pressure (ie, compressibility) when pressure is applied to the particles in a mold.

[0086] The particle size of the second particle 102 may be smaller than the particle size of the first particle 101. When the particle size of the second particle 102 is smaller than the particle size of the first particle 101, the second particle 102 is easily deformed. Therefore, the gap between two adjacent first particles 101 is easily filled with the second particle 102. As a result, the ion conductivity of the solid electrolyte 1000 is improved.

[0087] The thickness of the grain boundary layer 103 can be, for example, 10 nanometers or less. When the thickness of the grain boundary layer 103 is 10 nanometers or less, the bonding strength of the particles is stabilized at a high level, similar to the case of a microstructure formed by a conventional ceramic. Thus, the occurrence of particle delamination can be further suppressed, and a solid electrolyte 1000 having high ion conductivity can be obtained.

[0088] In order to improve the ion conductivity of the solid electrolyte 1000, the following formula may be satisfied.

[0089] 0.05≤(vp2+vgb) / (vp1+vp2+vgb)≤0.7

[0090] Here, vp1, vp2, and vgb are the volume of the first particle 101, the volume of the second particle 102, and the volume of the grain boundary layer 103, respectively.

[0091] In order to improve the ion conductivity of the solid electrolyte 1000 , the value of (vp2+vgb) / (vp1+vp2+vgb) may be 0.05 or more and 0.50 or less.

[0092] In order to improve the ion conductivity of the solid electrolyte 1000 , the value of (vp2+vgb) / (vp1+vp2+vgb) may be 0.05 or more and 0.30 or less.

[0093] In order to improve the ion conductivity of the solid electrolyte 1000 , the value of (vgb) / (vp2+vgb) may be 0.05 or more and 0.15 or less.

[0094] Hereinafter, an example of a method for producing a solid electrolyte in Embodiment 1 will be described in detail.

[0095] First, a production method will be described when the second particles 102 and the grain boundary layers 103 are composed of the same material group (ie, when the second solid electrolyte material and the third solid electrolyte material belong to the same material group).

[0096] A mixture of the powder of the first solid electrolyte material and the powder of the soft solid electrolyte material is pressurized to obtain a solid electrolyte having a microstructure including the second particles 102 and the grain boundary layer 103. The Young's modulus of the soft solid electrolyte material is lower than that of the first solid electrolyte material. In addition, the powder of the soft solid electrolyte material has a distribution in its crystallinity. The distribution of crystallinity will be described later.

[0097] The solid electrolyte material having a distribution in crystallinity (ie, a soft solid electrolyte material) eventually becomes the second solid electrolyte material and the third solid electrolyte material constituting the second particles 102 and the grain boundary layer 103 , respectively.

[0098] The powder of the soft solid electrolyte material having a distribution in crystallinity is roughly divided into a powder component having a low crystallinity and a remaining component.

[0099] The powder component having a low crystallinity spreads over the particle surfaces of the first particles 101 and bonds the particles together in the initial stage of pressurization. Thus, the grain boundary layer 103 is formed by the powder component having a low crystallinity.

[0100] The remaining components do not form the grain boundary layer 103. The remaining components finally have ion conductivity in the microstructure and constitute the second particles 102.

[0101] In this method, the generation of structural defects is suppressed, and the solid electrolyte 1000 having high ion conductivity is stably formed.

[0102] When the second particle 102 is composed of the same material group as the grain boundary layer 103, productivity is improved, and the structure of the solid electrolyte is easily stabilized from the viewpoint of bonding and thermal expansion between the second particle 102 and the grain boundary layer 103. In this case, the crystallinity of the first particle 101 is higher than that of the second particle 102, and the crystallinity of the second particle 102 is the same as or higher than that of the grain boundary layer 103. Generally, as the crystallinity increases, the ion conductivity is further improved, so the ion conductivity of the first particle 101 is higher than that of the second particle, and the ion conductivity of the second particle 102 is the same as or higher than that of the grain boundary layer 103.

[0103] Since the thermal expansion coefficient of the second particles is substantially the same as the thermal expansion coefficient of the grain boundary layer 103 , it is possible to obtain the solid electrolyte 1000 having high durability against thermal shock and thermal cycles.

[0104] Even when the second particles 102 and the grain boundary layer 103 are composed of the same material group, a mixture of powder of the first solid electrolyte material, powder of the second solid electrolyte material, and powder of the third solid electrolyte material can be prepared and then pressurized to obtain the solid electrolyte 1000.

[0105] Next, a production method in the case where the second particles 102 and the grain boundary layer 103 are formed of materials different from each other will be described.

[0106] A mixture of a powder of a first solid electrolyte material, a powder of a second solid electrolyte material, and a powder of a third solid electrolyte material is prepared, and then the mixture is pressurized to obtain the solid electrolyte 1000 .

[0107] The solid electrolyte 1000 may be formed using composite particles obtained by coating the surface of the first particle 101 with at least one selected from the second particle 102 and the grain boundary layer 103 .

[0108] The coating state can be confirmed by estimating the degree of composite formation based on the results of SEM observation or the change in specific surface area observed by the BET method.

[0109] (Implementation Method 2)

[0110] The power storage device of Embodiment 2 uses the solid electrolyte of Embodiment 1. In Embodiment 2, matters described in Embodiment 1 are omitted as appropriate.

[0111] The battery in the second embodiment includes a positive electrode, a negative electrode, and an electrolyte layer provided between the positive electrode and the negative electrode. At least one selected from the positive electrode, the negative electrode, and the electrolyte layer includes the solid electrolyte of the first embodiment.

[0112] Figure 2 2 is a cross-sectional view of a battery 2000 in Embodiment 2. Figure 2 As shown, the battery 2000 involved in the second embodiment includes a positive electrode 201, a negative electrode 203 and an electrolyte layer 202. The positive electrode 201 includes positive electrode active material particles 204 and the solid electrolyte 1000 in the first embodiment. The electrolyte layer 202 is arranged between the positive electrode 201 and the negative electrode 203. The electrolyte layer 202 is in contact with both the positive electrode 201 and the negative electrode 203. The electrolyte layer 202 includes the solid electrolyte 1000 in the first embodiment. The negative electrode 203 includes negative electrode active material particles 205 and the solid electrolyte 1000 in the first embodiment. The battery 2000 is, for example, an all-solid lithium secondary battery. The battery 2000 of the second embodiment includes the solid electrolyte 1000 described in the first embodiment, and therefore has a high energy density. The solid electrolyte 1000 of the first embodiment can suppress the occurrence of stratification, so the electrolyte layer 202 can be made thinner. Therefore, when the solid electrolyte 1000 in the first embodiment is used for the electrolyte layer 202, the energy density of the battery is further improved.

[0113] In Embodiment 2, each of the positive electrode 201, the negative electrode 203 and the electrolyte layer 202 may include the solid electrolyte 1000. The electrolyte layer 202 may include the solid electrolyte 1000 in Embodiment 1. Among the positive electrode 201, the negative electrode 203 and the electrolyte layer 202, the electrolyte layer 202 includes the largest amount of electrolyte material, so by using the solid electrolyte 1000 of Embodiment 1 for the electrolyte layer 202, the energy density is effectively improved. As long as at least one selected from the positive electrode 201, the negative electrode 203 and the electrolyte layer 202 includes the solid electrolyte 1000, the battery has a high energy density. Each of the positive electrode 201, the negative electrode 203 and the electrolyte layer 202 may include other solid electrolytes other than the solid electrolyte 1000 of Embodiment 1.

[0114] The positive electrode 201 contains a positive electrode active material, that is, a material that can absorb and release metal ions. Examples of metal ions include lithium ions. The positive electrode 201 contains, for example, a positive electrode active material (eg, positive electrode active material particles 204 ). The positive electrode 201 may contain a solid electrolyte 1000 .

[0115] Examples of positive electrode active materials include transition metal oxides containing lithium, transition metal oxides not containing lithium, transition metal fluorides, polyanionic materials, fluorinated polyanionic materials, transition metal sulfides, transition metal oxyfluorides, transition metal oxysulfides, or transition metal oxynitrides. When a transition metal oxide containing lithium is used as a positive electrode active material, the manufacturing cost of the battery 2000 can be reduced, and the average discharge voltage of the battery 2000 can be increased.

[0116] As a positive electrode active material, the positive electrode 201 may include at least one selected from Li(NiCoAl)O 2 and LiCoO 2 . These transition metal oxides can be used to increase the energy density of the battery 2000 .

[0117] In the positive electrode 201, the ratio of the volume vc1 of the positive electrode active material particles 204 to the total volume vc1 of the positive electrode active material particles 204 and the volume vc2 of the solid electrolyte 1000 is, for example, 30% or more and 95% or less. In other words, the volume ratio represented by the formula (vc1 / (vc1+vc2)) can be 0.3 or more and 0.95 or less. The ratio of the volume vc2 of the solid electrolyte 1000 to the total volume vc1 of the positive electrode active material particles 204 and the volume vc2 of the solid electrolyte 1000 is, for example, 5% or more and 70% or less. In other words, the volume ratio represented by the formula (vc2 / (vc1+vc2)) can be 0.05 or more and 0.70 or less. By appropriately adjusting the amount of the positive electrode active material particles 204 and the amount of the solid electrolyte 1000, the energy density of the battery 2000 can be fully ensured, and the battery 2000 can be operated at a high output.

[0118] The thickness of the positive electrode 201 may be not less than 10 μm and not more than 500 μm. By appropriately adjusting the thickness of the positive electrode 201, the energy density of the battery 2000 can be ensured, and the battery 2000 can be operated at a high output.

[0119] As described above, electrolyte layer 202 may contain solid electrolyte 1000 of Embodiment 1. Electrolyte layer 202 may contain not only solid electrolyte 1000 of Embodiment 1 but also a solid electrolyte other than the solid electrolyte of Embodiment 1.

[0120] Hereinafter, the solid electrolyte 1000 of the first embodiment is referred to as a first solid electrolyte. The solid electrolyte other than the solid electrolyte of the first embodiment is referred to as a second solid electrolyte.

[0121] When the electrolyte layer 202 contains not only the first solid electrolyte but also the second solid electrolyte, the first solid electrolyte and the second solid electrolyte may be uniformly dispersed in the electrolyte layer 202. The second solid electrolyte may have a composition different from that of the first solid electrolyte. The second solid electrolyte may have a structure different from that of the first solid electrolyte.

[0122] The thickness of the electrolyte layer 202 may be 1 μm or more and 500 μm or less. When the thickness of the electrolyte layer 202 is appropriately adjusted, short circuits between the positive electrode 201 and the negative electrode 203 can be reliably prevented, and the battery 2000 can be operated at high output.

[0123] The negative electrode 203 contains a negative electrode active material, that is, a material that can absorb and release metal ions. Examples of metal ions include lithium ions. The negative electrode 203 contains, for example, a negative electrode active material (eg, negative electrode active material particles 205 ). The negative electrode 203 may contain a solid electrolyte 1000 .

[0124] Examples of negative electrode active materials include metal materials, carbon materials, oxides, nitrides, tin compounds or silicon compounds. The metal material may be a single metal or an alloy. Examples of metal materials include lithium metal or lithium alloys. Examples of carbon materials include natural graphite, coke, carbon in graphitization, carbon fiber, spherical carbon, artificial graphite or amorphous carbon. From the viewpoint of capacity density, it is preferred to use at least one selected from silicon (i.e., Si), tin (i.e., Sn), silicon compounds and tin compounds as the negative electrode active material.

[0125] In the negative electrode 203, the ratio of the volume va1 of the negative electrode active material particles 205 to the total volume va1 of the negative electrode active material particles 205 and the volume va2 of the solid electrolyte 1000 is, for example, 30% or more and 95% or less. In other words, the volume ratio represented by the formula (va1 / (va1+va2)) can be 0.3 or more and 0.95 or less. The ratio of the volume va2 of the solid electrolyte 1000 to the total volume va1 of the negative electrode active material particles 105 and the volume va2 of the solid electrolyte 100 is, for example, 5% or more and 70% or less. In other words, the volume ratio represented by the formula (va2 / (va1+va2)) can be 0.05 or more and 0.70 or less. By appropriately adjusting the amount of the negative electrode active material particles 205 and the amount of the solid electrolyte 1000, the energy density of the battery 2000 can be fully ensured, and the battery 2000 can be operated at high output.

[0126] The thickness of the negative electrode 203 may be not less than 10 μm and not more than 500 μm. By appropriately adjusting the thickness of the negative electrode 203, the energy density of the battery 2000 can be sufficiently ensured, and the battery 2000 can be operated at a high output.

[0127] The second solid electrolyte may be a sulfide solid electrolyte. The sulfide solid electrolyte may be contained in the positive electrode 201, the negative electrode 203 and the electrolyte layer 202. Examples of sulfide solid electrolyte materials include Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, Li 3.25 Ge 0.25 P 0.75 S4 or Li 10 GeP2S 12 LiX (X is F, Cl, Br or I), Li2O, MO can be added to the sulfide solid electrolyte material. q or Li p MO q (M is P, Si, Ge, B, Al, Ga, In, Fe, or Zn, p is a natural number, and q is a natural number.) The sulfide solid electrolyte material improves the ion conductivity of the solid electrolyte 1000 .

[0128] The second solid electrolyte may be an oxide solid electrolyte. The oxide solid electrolyte may be contained in the positive electrode 201, the negative electrode 203, and the electrolyte layer 202. The oxide solid electrolyte material improves the ion conductivity of the solid electrolyte 1000.

[0129] Examples of oxide solid electrolytes are:

[0130] (i) NASICON-type solid electrolytes such as LiTi2(PO4)3 or its element substitution products,

[0131] (ii) (LaLi)TiO3-based perovskite solid electrolytes,

[0132] (iii)Li 14 ZnGe4O 16 , Li4SiO4, LiGeO4 or their element substitution bodies such as LISICON type solid electrolytes,

[0133] (iv)Li7La3Zr2O 12 or a garnet-type solid electrolyte such as an element substitution product thereof,

[0134] (v) Li3N or its H-substituted product, or

[0135] (vi) Li3PO4 or its N-substituted form.

[0136] The second solid electrolyte may be a halide solid electrolyte. The halide solid electrolyte may be contained in the positive electrode 201, the negative electrode 203, and the electrolyte layer 202. The halide solid electrolyte material improves the ion conductivity of the solid electrolyte 1000.

[0137] Examples of halide solid electrolytes include Li2MgX'4, Li2FeX'4, Li(Al,Ga,In)X'4, Li3(Al,Ga,In)X'6, LiOX' or LiX'. Wherein, X' is at least one element selected from F, Cl, Br and I. Examples of the halide solid electrolytes include Li3InBr6, Li3InCl6, Li2FeCl4, Li2CrCl4, Li3OCl or LiI.

[0138] The second solid electrolyte may be a complex hydride solid electrolyte. The complex hydride solid electrolyte may be included in the positive electrode 201, the negative electrode 203, and the electrolyte layer 202. The complex hydride solid electrolyte material improves the ion conductivity of the solid electrolyte 1000.

[0139] Examples of complex hydride solid electrolytes are LiBH4-LiI or LiBH4-P2S5.

[0140] The second solid electrolyte may be an organic polymer solid electrolyte. The organic polymer solid electrolyte may be contained in the positive electrode 201, the negative electrode 203, and the electrolyte layer 202. The organic polymer solid electrolyte material improves the ion conductivity of the solid electrolyte 1000.

[0141] Examples of organic polymer solid electrolytes include compounds of polymer compounds and lithium salts. The polymer compound may have an ethylene oxide structure. The polymer compound having an ethylene oxide structure can contain more lithium salts, thereby further improving the ion conductivity. Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9) or LiC(SO2CF3)3. One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used.

[0142] At least one selected from the positive electrode 201 , the negative electrode 203 , and the electrolyte layer 202 may include a non-aqueous electrolyte, a gel electrolyte, or an ionic liquid for the purpose of facilitating the transfer of lithium ions and improving the output characteristics of the battery 2000 .

[0143] The nonaqueous electrolyte contains a nonaqueous solvent and a lithium salt dissolved in the nonaqueous solvent.

[0144] Examples of the nonaqueous solvent include a cyclic carbonate solvent, a chain carbonate solvent, a cyclic ether solvent, a chain ether solvent, a cyclic ester solvent, a chain ester solvent or a fluorine solvent.

[0145] Examples of the cyclic carbonate solvent are ethylene carbonate, propylene carbonate or butylene carbonate.

[0146] Examples of the chain carbonate solvent are dimethyl carbonate, ethyl methyl carbonate or diethyl carbonate.

[0147] Examples of cyclic ether solvents are tetrahydrofuran, 1,4-dioxane or 1,3-dioxolane.

[0148] Examples of the chain ether solvent are 1,2-dimethoxyethane or 1,2-diethoxyethane.

[0149] An example of the cyclic ester solvent is γ-butyrolactone.

[0150] An example of the chain ester solvent is methyl acetate.

[0151] Examples of the fluorine solvent are fluoroethylene carbonate, fluoromethyl propionate, fluorobenzene, fluoroethyl methyl carbonate or fluorodimethyl carbonate.

[0152] One nonaqueous solvent selected from these may be used alone, or a mixture of two or more nonaqueous solvents selected from these may be used.

[0153] Examples of lithium salts are LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9) or LiC(SO2CF3)3.

[0154] One lithium salt selected from these may be used alone, or a mixture of two or more lithium salts selected from these may be used.

[0155] The concentration of the lithium salt may be 0.5 mol / liter or more and 2 mol / liter or less.

[0156] Examples of gel electrolytes include polymer materials impregnated with a non-aqueous electrolyte. Examples of polymer materials include polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, or polymethyl methacrylate. Other examples of polymer materials include polymers having ethyleneoxy groups.

[0157] Examples of cations contained in ionic liquids are:

[0158] (i) cations of aliphatic chain quaternary ammonium salts such as tetraalkylamine,

[0159] (ii) cations of aliphatic chain quaternary phosphonium salts such as tetraalkylphosphonium,

[0160] (iii) an aliphatic cyclic ammonium such as pyrrolidinium, morpholinium, imidazolinium, tetrahydropyrimidinium, piperazinium or piperidinium, or

[0161] (iv) Nitrogen-containing heterocyclic aromatic cations such as pyridinium and imidazolium.

[0162] Examples of anions that make up ionic liquids include PF6 - 、BF4 - 、SbF6 - 、AsF6 - 、SO3CF3 - 、N(SO2CF3)2 - 、N(SO2C2F5)2 - 、N(SO2CF3)(SO2C4F9) - or C(SO2CF3)3 - .

[0163] The ionic liquid may contain a lithium salt.

[0164] At least one selected from the positive electrode 201 , the negative electrode 203 , and the electrolyte layer 202 may contain a binder for the purpose of improving adhesion between particles.

[0165] Examples of binders include polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, polymethyl acrylate, polyethyl acrylate, polyhexyl acrylate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polyhexyl methacrylate, polyvinyl acetate, polyvinyl pyrrolidone, polyether, polyether sulfone, hexafluoropolypropylene, styrene-butadiene rubber or carboxymethyl cellulose.

[0166] Copolymers may also be used as binders. Examples of such binders include copolymers of two or more materials selected from tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid and hexadiene.

[0167] A mixture of two or more selected from the above materials may also be used as the binder.

[0168] At least one selected from the positive electrode 201 and the negative electrode 203 may contain a conductive auxiliary agent for the purpose of improving electronic conductivity.

[0169] Examples of conductive additives are:

[0170] (i) graphite such as natural graphite or synthetic graphite,

[0171] (ii) carbon black such as acetylene black or Ketjen black,

[0172] (iii) conductive fibers such as carbon fibers or metal fibers,

[0173] (iv) fluorinated carbons,

[0174] (v) Metal powders such as aluminum powder,

[0175] (vi) conductive whiskers such as zinc oxide whiskers or potassium titanate whiskers,

[0176] (vii) conductive metal oxides such as titanium oxide, or

[0177] (viii) Conductive polymer compounds such as polyaniline, polypyrrole or polythiophene.

[0178] The shape of the conductive auxiliary agent is not limited. Examples of the shape of the conductive auxiliary agent include needle-like, scale-like, spherical, or ellipsoidal. The conductive auxiliary agent may be in the form of particles.

[0179] The positive electrode active material particles 204 and the negative electrode active material particles 205 may also be coated with a coating material for the purpose of reducing the surface resistance. Only a portion of the surface of the positive electrode active material particles 204 may be coated with the coating material. Alternatively, the entire surface of the positive electrode active material particles 204 may be coated with the coating material. Similarly, only a portion of the surface of the negative electrode active material particles 205 may be coated with the coating material. Alternatively, the entire surface of the negative electrode active material particles 205 may be coated with the coating material.

[0180] Examples of coating materials include solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, halide solid electrolytes, polymer solid electrolytes, or complex hydride solid electrolytes. The coating material may be an oxide solid electrolyte. The oxide solid electrolyte has excellent high potential stability. By using an oxide solid electrolyte for the coating material, the charge and discharge efficiency of the battery 2000 is improved.

[0181] Examples of oxide solid electrolytes that can be used as coating materials include:

[0182] (i) Li-Nb-O compounds such as LiNbO3,

[0183] (ii) Li-BO compounds such as LiBO2 or Li3BO3,

[0184] (iii) Li-Al-O compounds such as LiAlO2,

[0185] (iv) Li-Si-O compounds such as Li4SiO4,

[0186] (v) Li2SO4,

[0187] (vi)Li4Ti5O 12 Li-Ti-O compounds such as

[0188] (vii) Li-Zr-O compounds such as Li2ZrO3,

[0189] (viii) Li-Mo-O compounds such as Li2MoO3,

[0190] (ix) Li-VO compounds such as LiV2O5, or

[0191] (x) Li-WO compounds such as Li2WO4.

[0192] Figure 3 FIG. 4 is a cross-sectional view of a battery 3000 according to a variation of Embodiment 2. Figure 3 As shown, the battery 3000 includes: a positive electrode including a positive electrode active material layer 301 and a current collector 303; a negative electrode including a negative electrode active material layer 302 and a current collector 303; and an electrolyte layer 304 provided between the positive electrode and the negative electrode. In the positive electrode, the positive electrode active material layer 301 is arranged on the current collector 303. In the negative electrode, the negative electrode active material layer 302 is arranged on the current collector 303. The electrolyte layer 304 includes the solid electrolyte in Embodiment 1.

[0193] The positive electrode active material layer 301 contains the positive electrode active material described above. The negative electrode active material layer 302 contains the negative electrode active material described above. The material of the current collector 303 is not limited as long as it has conductivity. As an example, the current collector 303 is made of a metal thin film such as copper foil.

[0194] Battery 3000 also includes the solid electrolyte of Embodiment 1, similarly to battery 2000 , and therefore has a high energy density.

[0195] (Example)

[0196] (Solid Electrolyte)

[0197] In this embodiment, the Figure 1 The solid electrolyte 1000 is shown.

[0198] As the first solid electrolyte material, an argyrodite-type sulfide was used. Specifically, a powder of a sulfide-based solid electrolyte Li6PS5Cl having an argyrodite structure (produced by Ampcera Corporation) was used.

[0199] As a material including the second solid electrolyte material and the third solid electrolyte material, a glass powder of Li2S-P2S5 (Li2S:P2S5=70:30 (molar ratio)) was used. Hereinafter, this glass powder is referred to as "LPS-based glass powder".

[0200] The LPS glass powder is annealed at 200 degrees Celsius. The annealed LPS glass powder contains triclinic crystals as a main component. The annealed LPS glass powder has a wide crystallinity distribution from crystalline to amorphous. The average particle size of the annealed LPS glass powder is 5 microns.

[0201] The annealed LPS glass powder was classified using an ultrasonic vibration sieve with a micro mesh having a maximum opening of 8 microns. The volume ratio of the LPS glass powder that passed through the micro mesh to the total LPS glass powder was approximately 0.1. The LPS glass powder that passed through the micro mesh contained many particles that did not undergo necking.

[0202] The LPS glass powder that passed through the microporous mesh was subjected to X-ray diffraction. No obvious peaks were observed in the X-ray diffraction pattern, so it was determined that the LPS glass powder that passed through the microporous mesh contained many particles that were not sintered and crystallized. In other words, it was determined that the powder that passed through the microporous mesh could be used as a material for the grain boundary layer 103.

[0203] Based on the classified structure, it is roughly determined that the components of the second particles 102 as a crystalline component account for 90 volume %, and the components of the grain boundary layer 103 as an amorphous component account for 10 volume %.

[0204] The weights of the powder of the sulfide solid electrolyte Li6PS5Cl having an argyrodite structure and the annealed LPS glass powder were measured in the ratios shown in Tables 1 and 2. These powders were then fully mixed with each other in an agate mortar under dry conditions for about 30 minutes to obtain a mixed powder in which these powders were uniformly dispersed.

[0205] Next, the mixed powder was placed in a mold. A uniaxial press was used to apply a pressure of 800 MPa to the mixed powder at a temperature of 120 degrees Celsius for 10 minutes to obtain a solid electrolyte consisting of a disc-shaped pressed powder sample. The solid electrolyte was taken out of the mold. In this way, a solid electrolyte was obtained.

[0206] Then, the effective ion conductivity of the obtained solid electrolyte is measured as follows. As described in the embodiment, the ion conductivity of the solid electrolyte measured under high pressure is significantly different from the ion conductivity of the solid electrolyte measured under atmospheric pressure. As shown below, in the embodiment, the ion conductivity of the solid electrolyte contained in the battery is measured as the effective ion conductivity.

[0207] The first indium foil and the second indium foil are respectively arranged on the upper surface and the lower surface of the solid electrolyte. The thickness of the first indium foil and the second indium foil is 50 micrometers. Then, pressure is applied between the upper surface and the lower surface of the solid electrolyte through the first indium foil and the second indium foil. Thus, the first indium foil and the second indium foil are respectively bonded to the upper surface and the lower surface of the solid electrolyte. Finally, the solid electrolyte is released from the pressure. In this way, a battery having the first indium foil, the solid electrolyte and the second indium foil is obtained.

[0208] Then, the battery was placed in a constant temperature bath maintained at 25°C ± 1°C.

[0209] The atmosphere inside the thermostatic bath is the air atmosphere. The pressure inside the thermostatic bath is the atmospheric pressure.

[0210] The battery was placed in a thermostatic chamber, and in this state, the impedance of the solid electrolyte was measured at a measurement frequency of 110 Hz to 10 MHz through the first and second indium foils using an impedance measurement system (manufactured by Solartron Co., Ltd., product name: 12608W), and the effective ion conductivity of the solid electrolyte contained in the battery was calculated.

[0211] Tables 1 and 2 show the effective ion conductivities of the solid electrolytes of Samples 1 to 7.

[0212] (Secondary battery)

[0213] The following is a description of a method for manufacturing a secondary battery. Figure 3 A secondary battery 3000 is shown.

[0214] First, a positive electrode paste, a negative electrode paste, and an electrolyte paste are prepared.

[0215] (Positive electrode paste)

[0216] The positive electrode paste contains a solid electrolyte material and a positive electrode active material.

[0217] The solid electrolyte material is a crystallized glass powder of a sulfide-based solid electrolyte Li6PS5Cl of the argyrodite type. The average particle size of the crystallized glass powder is 2 microns. The ion conductivity of the sulfide-based solid electrolyte Li6PS5Cl is approximately 2mS / cm to 3mS / cm.

[0218] The positive electrode active material is composed of the chemical formula LiNi 0.8 Co 0.15 Al 0.05 Powder of a layered LiNiCoAl composite oxide represented by O2. The average particle size of the layered LiNiCoAl composite oxide is approximately 5 micrometers.

[0219] The positive electrode paste was prepared as follows.

[0220] The solid electrolyte material and the positive electrode active material are mixed with each other and then uniformly dispersed to obtain a mixture. Next, a hydrogenated styrene-based thermoplastic elastomer (hereinafter referred to as "SEBS") and tetralin are added to the mixture, and then the mixture is fully stirred for about 20 minutes at room temperature (i.e., approximately 25 degrees Celsius) using a rotary mixer at a rotation speed of 1600 rpm to obtain a positive electrode paste. SEBS and tetralin are used as an organic binder and a solvent, respectively.

[0221] (Negative electrode paste)

[0222] The negative electrode paste also contains a solid electrolyte material and a negative electrode active material.

[0223] As in the case of the positive electrode paste, the solid electrolyte material is a crystallized glass powder of a sulfide-based solid electrolyte Li6PS5Cl of the argyrodite type. The average particle size of the crystallized glass powder is 2 microns.

[0224] The negative electrode active material is natural graphite powder with an average particle size of approximately 10 microns.

[0225] The negative electrode paste is prepared in the same manner as the positive electrode paste.

[0226] (Electrolyte paste)

[0227] SEBS and tetralin were added to the solid electrolytes of samples 1 to 7, and then the mixture was stirred thoroughly for about 20 minutes at room temperature (i.e., approximately 25 degrees Celsius) using a rotary mixer at 1600 rpm to obtain an electrolyte paste. SEBS and tetralin were used as an organic binder and a solvent, respectively.

[0228] The positive electrode paste was applied to a copper foil having a thickness of approximately 20 micrometers by screen printing. The applied positive electrode paste was dried under vacuum at approximately 100 degrees Celsius for 1 hour to form a positive electrode active material layer 301 on the copper foil. The copper foil functions as a current collector 303. The thickness of the positive electrode active material layer 301 is approximately 60 micrometers.

[0229] Next, the electrolyte paste is applied onto the positive electrode active material layer 301 using a metal mask and a doctor blade. The thickness of the applied electrolyte paste is approximately 100 μm. The electrolyte paste is then dried at approximately 100° C. under vacuum for 1 hour. In this way, a positive electrode having an electrolyte layer 304 formed on the surface is obtained.

[0230] The surface of the electrolyte layer 304 was observed using an optical microscope at a magnification of 50. As a result, no cracks were observed on the surface of the electrolyte layer 304.

[0231] The copper foil formed with the electrolyte layer 304 is carefully handled so that impact and deformation that may cause structural defects inside the electrolyte layer 304 are not applied to the electrolyte layer 304 .

[0232] The negative electrode paste was applied to a copper foil having a thickness of approximately 20 micrometers by screen printing. The applied negative electrode paste was dried under vacuum at approximately 100°C for 1 hour to form a negative electrode active material layer 302 on the copper foil. The copper foil served as a current collector 303. The thickness of the negative electrode active material layer 302 was approximately 80 micrometers.

[0233] Next, a negative electrode having an electrolyte layer 304 formed on the surface was obtained in the same manner as in the case of the positive electrode. No cracks were observed on the surface of the electrolyte layer 304 of the negative electrode.

[0234] Then, the positive electrode and the negative electrode are stacked in such a way that the surface of the electrolyte layer 304 of the positive electrode is in contact with the surface of the electrolyte layer 304 of the negative electrode. In this way, a stacked body is obtained. Elastic sheets are stacked on the upper and lower surfaces of the stacked body. These elastic sheets have 5×10 6 Pa and a thickness of 70 microns. Next, the laminate was placed in a mold. The laminate was pressurized for 100 seconds at a pressure of 800 MPa in the mold while the laminate was heated to 50°C. The laminate was removed from the mold and the two elastomer sheets were carefully removed without damaging the laminate. In this way, a secondary battery with a rectangular shape was obtained.

[0235] The lead terminal is bonded to the surface of the current collector 303 (ie, copper foil) of the secondary battery using an Ag-based highly conductive bonding agent to attach a terminal electrode.

[0236] The charge and discharge characteristics (ie, charge capacity, discharge capacity, and charge and discharge efficiency) of the secondary battery were evaluated. In other words, the charge capacity, discharge capacity, and charge and discharge efficiency in the initial measurement were measured at 0.05C at room temperature (ie, approximately 25 degrees Celsius).

[0237] In addition, the cross section of the secondary battery was observed. Specifically, the secondary battery was cut using a Thomson blade to expose the cross section of the central portion of the secondary battery. An optical microscope was used to observe the entire exposed cross section at a magnification of 50 times to determine whether the internal structure of the secondary battery had structural defects such as stratification. In each sample, 5 secondary batteries were used for cross-sectional observation. These results are shown in Tables 1 and 2. In the "Structural Defects" column in Tables 1 and 2, the number of secondary batteries in which structural defects were observed in the cross section among the 5 secondary batteries is shown as the numerator. The denominator is, of course, 5.

[0238] Table 1

[0239]

[0240] Table 2

[0241]

[0242] Comparing Samples 2 to 6 with Samples 1 and 7, it can be seen that by making the first particle component (i.e., argyrodite-type sulfide) contain LPS-based glass powder, a battery with no structural defects and a high effective ion conductivity of more than 1.98 mS / cm can be obtained.

[0243] The inventors believe that since the battery has no structural defects, delamination during pressurization is suppressed. Note that the LPS-based glass powder constitutes the second particles 102 and the grain boundary layer 103 (second particles 102: grain boundary layer 103 = 90 volume %: 10 volume %).

[0244] The charge capacity of the secondary batteries of Samples 2 to 6 was greater than 200 mAh / g. In addition, the secondary batteries of Samples 2 to 6 had higher charge and discharge efficiencies than those of Samples 1 and 7 (ie, charge and discharge efficiencies of approximately 80% or more).

[0245] Thus, the secondary batteries of Samples 2 to 6 had a charge capacity greater than 200 mAh / g and a charge and discharge efficiency of 80% or more.

[0246] The results of Samples 2 to 3 and Samples 4 to 6 show that the secondary battery has a high ion conductivity of 1.98 mS / cm or more and has no structural defects even when the LPS-based glass powder has a volume ratio of 30% or more.

[0247] By comparing samples 2 to 4 with samples 5 to 6, it can be seen that when the LPS-based glass powder has a volume ratio of less than 50% (preferably 5% or more and less than 50%, more preferably 5% or more and less than 30%), the secondary battery has a high ion conductivity of approximately 4 mS / cm or more.

[0248] On the other hand, the results of Sample 7 show that when the solid electrolyte contains LPS-based glass powder but does not contain argyrodite-type sulfide, although no structural defects occur, the solid electrolyte has low effective ion conductivity and low charge and discharge efficiency. This is because the secondary battery of Sample 7 does not contain argyrodite-type sulfide. Note that argyrodite-type sulfide functions as an ion conduction path.

[0249] The results of Sample 1 show that when the solid electrolyte contains argyrodite-type sulfide but does not contain LPS-based glass powder, the solid electrolyte has low effective ion conductivity and low charge and discharge efficiency. This is because the secondary battery of Sample 1 does not contain LPS-based glass powder.

[0250] Industrial Availability

[0251] The solid electrolyte disclosed herein can be used in a secondary battery. The secondary battery can be used in electronic equipment or automobiles.

[0252] Description of Reference Numerals

[0253] 1000 Solid Electrolyte

[0254] 101 The 1st Particle

[0255] 102 The 2nd Particle

[0256] 103 Grain boundary layer

[0257] 2000 Secondary Batteries

[0258] 201 Positive electrode

[0259] 202 electrolyte layer

[0260] 203 Negative electrode

[0261] 204 Positive electrode active material particles

[0262] 205 Negative electrode active material particles

[0263] 3000 Secondary battery

[0264] 301 positive electrode active material layer

[0265] 302 Negative electrode active material layer

[0266] 303 Current Collector

[0267] 304 electrolyte layer

Claims

1. A solid electrolyte comprising: first particles composed of a first solid electrolyte material; second particles composed of a second solid electrolyte material; and A grain boundary layer composed of a third solid electrolyte material, The first solid electrolyte material has a higher ion conductivity than the second solid electrolyte material, and The second solid electrolyte material has a lower Young's modulus than the first solid electrolyte material.

2. The solid electrolyte according to claim 1, The first solid electrolyte material includes at least one selected from the group consisting of sulfides, oxides, and halides.

3. A solid electrolyte comprising: first particles composed of a first solid electrolyte material; and second particles composed of a second solid electrolyte material, The first solid electrolyte material has a higher ion conductivity than the second solid electrolyte material, and The second solid electrolyte material has a lower Young's modulus than the first solid electrolyte material, The first solid electrolyte material includes at least one selected from the group consisting of sulfides and halides.

4. The solid electrolyte according to claim 2 or 3, The first solid electrolyte material includes argyrodite-type sulfide.

5. The solid electrolyte according to claim 4, The argyrodite-type sulfide has a composition formula of Li α PS β Cl γ express, in, 5.5≤α≤6.5, 4.5≤β≤5.5, 0.5≤γ≤1.

5.

6. The solid electrolyte according to any one of claims 1 to 3, The second solid electrolyte material includes at least one selected from the group consisting of sulfides, oxides, and halides.

7. The solid electrolyte according to claim 6, The second solid electrolyte material is selected from sulfides, and The sulfide includes lithium sulfide and phosphorus sulfide.

8. The solid electrolyte according to claim 7, The sulfide contains Li p SP q S 5 , Satisfies the following two equations, 1.5≤p≤2.5 and 1.5≤q≤2.

5.

9. The solid electrolyte according to claim 6, The second solid electrolyte material includes a glassy sulfide having triclinic crystals as a main component.

10. The solid electrolyte according to any one of claims 1 to 3, The thickness of the grain boundary layer is smaller than the particle size of the first particle and the particle size of the second particle, and The Young's modulus of the third solid electrolyte material is less than or equal to the Young's modulus of the second solid electrolyte material.

11. The solid electrolyte according to claim 10, The third solid electrolyte material has a lower Young's modulus than the second solid electrolyte material.

12. The solid electrolyte according to claim 10, The third solid electrolyte material has lower crystallinity than the second solid electrolyte material.

13. The solid electrolyte according to claim 10, The third solid electrolyte material is amorphous.

14. The solid electrolyte according to claim 10, wherein the second solid electrolyte material comprises at least one selected from the group consisting of sulfides, oxides, and halides. The third solid electrolyte material belongs to the same material group as the second solid electrolyte material.

15. The solid electrolyte according to claim 10, The grain boundary layer exists between the first particle and the second particle.

16. The solid electrolyte according to claim 15, The grain boundary layer exists between two adjacent first particles, and The grain boundary layer exists between two of the second particles adjacent to each other.

17. The solid electrolyte according to claim 10, Satisfies the following formula, 0.05≤(vp2+vgb) / (vp1+vp2+vgb)≤0.7, in, vp1, vp2, and vgb are the volume of the first particle, the volume of the second particle, and the volume of the grain boundary layer, respectively.

18. The solid electrolyte according to claim 17, Satisfies the following formula, 0.05≤(vp2+vgb) / (vp1+vp2+vgb)≤0.

5.

19. The solid electrolyte according to claim 18, Satisfies the following formula, 0.05≤(vp2+vgb) / (vp1+vp2+vgb)≤0.

3.

20. The solid electrolyte according to claim 10, Satisfies the following formula, 0.05≤(vgb) / (vp2+vgb)≤0.15, in, vp2 and vgb are the volume of the second particle and the volume of the grain boundary layer, respectively.

21. A battery comprising a positive electrode, a negative electrode, and an electrolyte layer disposed between the positive electrode and the negative electrode, At least one selected from the positive electrode, the negative electrode, and the electrolyte layer includes the solid electrolyte according to any one of claims 1 to 20.

22. The battery according to claim 21, The electrolyte layer includes the solid electrolyte.