A battery back passivation structure and manufacturing method thereof, and solar cell
By depositing a doped passivation layer and an internal reflective layer on the back of the silicon wafer of the solar cell, the problem of poor passivation ability of a single layer of silicon nitride oxide film in the existing technology is solved, and a more efficient preparation process and better performance are achieved. battery performance.
Patent Information
- Application Number
- CN202111056381.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-09
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-09-09
AI Technical Summary
The existing back passivation structure of solar cells deposits an aluminum oxide film layer or a silicon nitride oxide film layer on the back of the silicon wafer. The single-layer passivation ability is poor, resulting in long preparation time, low efficiency, and increased winding plating/back field boat printing, etc. bad.
The doping gas and the first reaction gas are used to deposit the doped passivation layer in the coating equipment, and the internal reflection layer is directly or indirectly deposited on the doped passivation layer away from the silicon wafer surface, and the PECVD process is used to reduce the preparation steps and damage. Enhance passivation capabilities.
The passivation ability of the battery back passivation structure is improved, the preparation time is shortened, adverse phenomena are reduced, and the efficiency of the solar cell is improved.
Smart Images

Figure CN113782638B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of photovoltaic technology, and in particular to a battery back passivation structure and a manufacturing method thereof, and a solar cell. Background Art
[0002] Solar cells are devices that can convert solar energy into electrical energy. In order to improve the efficiency of solar cells, back passivation technology came into being. At present, the back passivation structure of solar cells is to deposit an aluminum oxide film or a silicon oxynitride film on the back of the silicon wafer. The single-layer back passivation film has poor passivation ability and a single-layer silicon oxynitride film is thick, resulting in a long preparation time and low preparation efficiency. At the same time, it will also increase defects such as wrap-around plating / back field boat printing.
[0003] Therefore, how to solve the above technical problems should be the focus of technical personnel in this field. Summary of the invention
[0004] The purpose of the present application is to provide a battery back passivation structure and a manufacturing method thereof, and a solar cell, so as to improve the passivation ability of the battery back passivation structure, shorten the preparation process time and improve the battery yield.
[0005] In order to solve the above technical problems, the present application provides a method for manufacturing a battery back passivation structure, comprising:
[0006] Introducing doping gas and first reaction gas into the coating equipment to deposit a doped passivation layer on the back side of the silicon wafer;
[0007] A second reaction gas is introduced into the coating device to directly or indirectly deposit an internal reflection layer on the surface of the doped passivation layer away from the silicon wafer.
[0008] Optionally, after depositing the doped passivation layer on the back side of the silicon wafer, the method further comprises:
[0009] Introducing the first reaction gas into the coating device to deposit a silicon oxynitride layer on the surface of the doped passivation layer away from the silicon wafer;
[0010] Accordingly, indirectly depositing an internal reflection layer on a surface of the doped passivation layer away from the silicon wafer comprises:
[0011] An internal reflection layer is deposited on a surface of the silicon oxynitride layer away from the doped passivation layer.
[0012] Optionally, the first reaction gas includes SiH4, NH3 and N2O, and the doped passivation layer is a doped silicon oxynitride layer; the second reaction gas includes SiH4 and NH3, and the internal reflection layer is a silicon nitride layer.
[0013] Optionally, depositing an internal reflection layer on a surface of the silicon oxynitride layer away from the doped passivation layer comprises:
[0014] A plurality of internal reflection layers stacked in sequence are deposited on a surface of the silicon oxynitride layer away from the doped passivation layer, and the doping gas includes a gas containing phosphorus, boron, aluminum, gallium, and indium.
[0015] Optionally, in a direction away from the silicon wafer, the refractive index of the multiple internal reflection layers stacked in sequence gradually decreases.
[0016] Optionally, the number of layers of the internal reflection layer is three.
[0017] Optionally, in the direction away from the silicon oxynitride layer, the refractive index of the first layer of the internal reflection layer is between 2.35 and 2.25, and the thickness is between 10nm and 35nm; the refractive index of the second layer of the internal reflection layer is between 2.25 and 2.1, and the thickness is between 10nm and 20nm; the refractive index of the third layer of the internal reflection layer is between 2.1 and 1.9, and the thickness is between 10nm and 20nm.
[0018] Optionally, before introducing the doping gas and the first reaction gas into the coating device and depositing the doped passivation layer on the back side of the silicon wafer, the method further includes:
[0019] The silicon wafer is subjected to acid polishing or alkaline polishing.
[0020] The present application also provides a battery back passivation structure, and the battery back passivation structure is manufactured by any of the battery back passivation structure manufacturing methods described above.
[0021] The present application also provides a solar cell, which includes the above-mentioned cell back passivation structure.
[0022] The present application provides a method for manufacturing a back passivation structure of a battery, comprising: introducing a doping gas and a first reaction gas into a coating device to deposit a doped passivation layer on the back side of a silicon wafer; introducing a second reaction gas into the coating device to directly or indirectly deposit an internal reflection layer on a surface of the doped passivation layer away from the silicon wafer.
[0023] It can be seen that the battery back passivation structure in the present application includes a doped passivation layer and an internal reflection layer stacked on the back of the silicon wafer, and the passivation ability is enhanced; in the present application, when depositing the doped passivation layer, the doping gas and the first reaction gas are simultaneously introduced into the coating equipment for deposition, that is, the doped passivation layer is obtained by one step, avoiding the method of first depositing the passivation layer and then doping the passivation layer by diffusion or ion implantation, shortening the preparation time of the doped passivation layer, and avoiding the diffusion or ion implantation process causing damage to the passivation layer, affecting the performance of the back passivation structure; since the deposited doped passivation layer has a strong passivation performance, the thickness of the doped passivation layer can be thinned, shortening the preparation process time, and thus reducing defects such as wrap-around plating / back field boat printing.
[0024] In addition, the present application also provides a cell back passivation structure and a solar cell having the above advantages. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions of the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0026] Figure 1 A flow chart of a method for manufacturing a battery back passivation structure provided in an embodiment of the present application;
[0027] Figure 2 A flow chart of another method for manufacturing a battery back passivation structure provided in an embodiment of the present application;
[0028] Figure 3 A schematic diagram of a battery back passivation structure provided in an embodiment of the present application. DETAILED DESCRIPTION
[0029] In order to enable those skilled in the art to better understand the present application, the present application is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0030] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0031] As described in the background technology section, the current back passivation structure of solar cells is to deposit an aluminum oxide film layer or a silicon oxynitride film layer on the back of the silicon wafer. The single-layer back passivation film layer has poor passivation ability and the single-layer silicon oxynitride film layer is thick, resulting in a long preparation time and low preparation efficiency. At the same time, it will also increase defects such as wrap-around plating / back field boat printing.
[0032] In view of this, the present application provides a method for manufacturing a battery back passivation structure, please refer to Figure 1 , Figure 1 A flow chart of a method for manufacturing a battery back passivation structure provided in an embodiment of the present application, the method comprising:
[0033] Step S101: introducing a doping gas and a first reaction gas into a coating device to deposit a doped passivation layer on the back side of a silicon wafer.
[0034] In order to ensure the performance of the doped passivation layer, the doped passivation layer is generally deposited by plasma enhanced chemical vapor deposition (PECVD), and the corresponding coating equipment is PECVD equipment.
[0035] It should be noted that the type of PECVD equipment is not specifically limited in this application and can be selected at will. For example, a plate-type PECVD equipment or a tubular PECVD equipment can be used.
[0036] The doping gas includes the doping elements required in the doping type passivation layer, and the specific gas type depends on the doping elements.
[0037] The first reaction gas refers to the gas required for depositing and forming the non-doped passivation layer, and the specific gas type depends on the material of the passivation layer.
[0038] It should be noted that the doped passivation layer is not limited in the present application and can be set at will. For example, the doped passivation layer can be a doped silicon nitride layer or a doped silicon oxynitride layer. In the present application, there is no need to deposit an aluminum oxide layer, and the atomic layer deposition process for preparing the aluminum oxide layer is omitted. Only the plasma enhanced chemical vapor deposition process is required, which reduces the idle time of the semi-finished product of the back passivation structure in the workshop and the fragmentation rate and other defects caused during the process.
[0039] Preferably, the doped passivation layer is a doped silicon oxynitride layer. After annealing, the doped silicon oxynitride layer has more fixed negative charges and a longer minority carrier lifetime than the doped silicon nitride layer, so that the performance of the battery back passivation structure is better. At this time, the first reaction gas includes SiH4, NH3 and N2O. The second reaction gas includes SiH4 and NH3, and the internal reflection layer is a silicon nitride layer.
[0040] When the doped passivation layer is a doped silicon nitride layer, the first reaction gas includes SiH 4 and NH 3 .
[0041] Compared with the aluminum oxide layer, the doped silicon oxynitride layer contains more H and has an enhanced H passivation ability; the doped silicon oxynitride layer combines the advantages of the aluminum oxide layer and the silicon oxynitride surface passivation and has an enhanced surface passivation ability; compared with a single-layer silicon oxynitride layer, the doped silicon oxynitride layer has an enhanced field passivation ability, thereby improving the efficiency of the solar cell.
[0042] It should be noted that the doping elements are not limited in the present application and may be used as appropriate. For example, the doping elements may be group 3A elements (such as boron, aluminum, gallium, indium) or group 5A elements (such as phosphorus, arsenic), and correspondingly, the doping gas may be B2H6, TMA (trimethylaluminum), TMGa (trimethylgallium), PH3, etc. In addition to the required doping elements, the doping gas will not cause doping of other elements to the doped passivation layer.
[0043] Step S102: introducing a second reaction gas into the coating device to directly or indirectly deposit an internal reflection layer on the surface of the doped passivation layer away from the silicon wafer.
[0044] Direct deposition means that after depositing the doped passivation layer, an internal reflection layer is deposited directly on the surface of the doped passivation layer away from the silicon wafer. Indirect deposition means that after depositing the doped passivation layer, a silicon oxynitride layer is first deposited on the surface of the doped passivation layer away from the silicon wafer, and then an internal reflection layer is deposited on the surface of the silicon oxynitride layer. See below for details. The internal reflection layer is generally a silicon nitride layer, and accordingly, the second reaction gas includes SiH4 and NH3.
[0045] It should be pointed out that the number of the internal reflection layer can be one layer or multiple layers, which is not limited in the present application.
[0046] The battery back passivation structure in the present application includes a doped passivation layer and an internal reflection layer stacked on the back of a silicon wafer, and the passivation ability is enhanced; in the present application, when depositing the doped passivation layer, the doping gas and the first reaction gas are simultaneously introduced into the coating equipment for deposition, that is, the doped passivation layer is obtained by one step, avoiding the method of first depositing the passivation layer and then doping the passivation layer by diffusion or ion implantation, shortening the preparation time of the doped passivation layer, and avoiding the diffusion or ion implantation process causing damage to the passivation layer, thereby affecting the performance of the back passivation structure; since the deposited doped passivation layer has a strong passivation performance, the thickness of the doped passivation layer can be thinned, shortening the preparation process time, and thus reducing defects such as wrap-around plating / back field boat printing.
[0047] Please refer to Figure 2 , Figure 2A flowchart of another method for manufacturing a battery back passivation structure provided in an embodiment of the present application, the method comprising:
[0048] Step S201: introducing a doping gas and a first reaction gas into a coating device to deposit a doped passivation layer on the back side of a silicon wafer.
[0049] In this step, the doped passivation layer is a doped silicon oxynitride layer.
[0050] Step S202: introducing the first reaction gas into the coating device to deposit a silicon oxynitride layer on the surface of the doped passivation layer away from the silicon wafer.
[0051] In this embodiment, a silicon oxynitride layer is deposited between the doped silicon oxynitride layer and the internal reflection layer. The silicon oxynitride layer is rich in H and can provide a certain H passivation, further enhancing the H passivation ability of the back passivation structure, thereby further improving the efficiency of the solar cell; and when the doped silicon oxynitride layer is relatively thin, it can also provide a certain surface passivation.
[0052] The refractive index of the silicon oxynitride layer is greater than that of the doped silicon oxynitride layer. The refractive index of the doped silicon oxynitride layer is controlled between 1.4 and 1.8, and the thickness of the doped silicon oxynitride layer is between 10 and 50 nm. The refractive index of the silicon oxynitride layer is between 1.6 and 1.9, and the thickness of the silicon oxynitride layer is between 10 and 20 nm.
[0053] Step S203: introducing a second reaction gas into the coating device to deposit an internal reflection layer on the surface of the silicon oxynitride layer away from the doped passivation layer.
[0054] As an practicable manner, depositing an internal reflection layer on a surface of the silicon oxynitride layer away from the doped passivation layer comprises:
[0055] A plurality of internal reflection layers stacked in sequence are deposited on a surface of the silicon oxynitride layer away from the doped passivation layer, and the doping gas includes a gas containing phosphorus, boron, aluminum, gallium, and indium.
[0056] In the direction away from the silicon wafer, the refractive index of the multiple layers of internal reflection layers stacked in sequence gradually decreases, which can enhance the passivation performance of the back passivation structure, reduce the reflectivity of the back surface, optimize the anti-reflection effect of the internal reflection layer and the passivation effect with the body surface. The refractive index of the internal reflection layer located at the silicon oxynitride layer away from the silicon wafer surface is the largest, and it has a better body surface passivation effect, further improving the open circuit voltage of the solar cell.
[0057] The number of internal reflection layers includes but is not limited to three, four, five, and the like.
[0058] When the number of internal reflection layers is three, in the direction away from the silicon oxynitride layer, the refractive index of the first internal reflection layer is between 2.35 and 2.25, and the thickness is between 10nm and 35nm; the refractive index of the second internal reflection layer is between 2.25 and 2.1, and the thickness is between 10nm and 20nm; the refractive index of the third internal reflection layer is between 2.1 and 1.9, and the thickness is between 10nm and 20nm. When the number of internal reflection layers is three, the schematic diagram of the back passivation structure of the battery is as follows Figure 3 As shown, from top to bottom are a silicon wafer 1, a doped silicon oxynitride layer 2, a silicon oxynitride layer 3, and a three-layer stacked silicon nitride layer 4.
[0059] Based on any of the above embodiments, in one embodiment of the present application, the doping gas and the first reaction gas are introduced into the coating device, and before the doped passivation layer is deposited on the back side of the silicon wafer, the method further includes:
[0060] The silicon wafer is subjected to acid polishing or alkaline polishing to remove damage on the surface of the silicon wafer.
[0061] The specific polishing process is well known to those skilled in the art and will not be described in detail here.
[0062] The following uses different doping elements and the PECVD method as an example to illustrate the method for manufacturing the battery back passivation structure in this application.
[0063] Example 1
[0064] Step 1, performing acid polishing and etching on the silicon wafer;
[0065] Step 2, using PH3, SiH4, NH3 and N2O, a total of four special gases, to pass into the PECVD equipment to produce a phosphorus-doped silicon oxynitride layer, the refractive index of the phosphorus-doped silicon oxynitride layer is controlled between 1.4 and 1.8, and the thickness of the phosphorus-doped silicon oxynitride layer is between 10 and 50 nm;
[0066] Step 3: On the surface of the phosphorus-doped silicon oxynitride layer, a silicon oxynitride layer is deposited using three special gases, SiH4, NH3 and N2O, wherein the refractive index of the silicon oxynitride layer is between 1.6 and 1.9, and the thickness of the silicon oxynitride layer is controlled to be between 10 and 20 nm;
[0067] Step 4: On the surface of the silicon nitride oxide layer, a first silicon nitride layer is made by using two special gases, SiH4 and NH3, with a refractive index between 2.35 and 2.25, and a thickness of the first silicon nitride layer is controlled between 10 and 35 nm;
[0068] Step 5: On the surface of the first silicon nitride layer, a second silicon nitride layer is made by using two special gases, SiH4 and NH3, with a refractive index between 2.25 and 2.1, and a thickness of the second silicon nitride layer is controlled between 10 and 20 nm;
[0069] Step 6: On the surface of the second silicon nitride layer, use SiH4 and NH3 as two special gases to make a third silicon nitride layer with a refractive index between 2.1 and 1.9. The thickness of the third silicon nitride layer is controlled at 10 to 20 nm.
[0070] Example 2
[0071] Step 1, performing acid polishing and etching on the silicon wafer;
[0072] Step 2, using B2H6, SiH4, NH3 and N2O, a total of four special gases, to pass into the PECVD equipment to produce a boron-doped silicon oxynitride layer, the refractive index of the boron-doped silicon oxynitride layer is controlled between 1.4 and 1.8, and the thickness of the boron-doped silicon oxynitride layer is between 10 and 50 nm;
[0073] Step 3: On the surface of the boron-doped silicon oxynitride layer, a silicon oxynitride layer is deposited using three special gases, SiH4, NH3 and N2O, wherein the refractive index of the silicon oxynitride layer is between 1.6 and 1.9, and the thickness of the silicon oxynitride layer is controlled to be between 10 and 20 nm;
[0074] Step 4: On the surface of the silicon nitride oxide layer, a first silicon nitride layer is made by using two special gases, SiH4 and NH3, with a refractive index between 2.35 and 2.25, and a thickness of the first silicon nitride layer is controlled between 10 and 35 nm;
[0075] Step 5: On the surface of the first silicon nitride layer, a second silicon nitride layer is made by using two special gases, SiH4 and NH3, with a refractive index between 2.25 and 2.1, and a thickness of the second silicon nitride layer is controlled between 10 and 20 nm;
[0076] Step 6: On the surface of the second silicon nitride layer, use SiH4 and NH3 as two special gases to make a third silicon nitride layer with a refractive index between 2.1 and 1.9. The thickness of the third silicon nitride layer is controlled at 10 to 20 nm.
[0077] Example 3
[0078] Step 1, performing acid polishing and etching on the silicon wafer;
[0079] Step 2, using TMGa, SiH4, NH3 and N2O, a total of four special gases, to pass into the PECVD equipment to produce a gallium-doped silicon oxynitride layer, the refractive index of the gallium-doped silicon oxynitride layer is controlled between 1.4 and 1.8, and the thickness of the gallium-doped silicon oxynitride layer is between 10 and 50 nm;
[0080] Step 3: On the surface of the gallium-doped silicon oxynitride layer, a silicon oxynitride layer is deposited using three special gases, SiH4, NH3 and N2O, wherein the refractive index of the silicon oxynitride layer is between 1.6 and 1.9, and the thickness of the silicon oxynitride layer is controlled to be between 10 and 20 nm;
[0081] Step 4: On the surface of the silicon nitride oxide layer, a first silicon nitride layer is made by using two special gases, SiH4 and NH3, with a refractive index between 2.35 and 2.25, and a thickness of the first silicon nitride layer is controlled between 10 and 35 nm;
[0082] Step 5: On the surface of the first silicon nitride layer, a second silicon nitride layer is made by using two special gases, SiH4 and NH3, with a refractive index between 2.25 and 2.1, and a thickness of the second silicon nitride layer is controlled between 10 and 20 nm;
[0083] Step 6: On the surface of the second silicon nitride layer, use SiH4 and NH3 as two special gases to make a third silicon nitride layer with a refractive index between 2.1 and 1.9. The thickness of the third silicon nitride layer is controlled at 10 to 20 nm.
[0084] Example 4
[0085] Step 1, performing acid polishing and etching on the silicon wafer;
[0086] Step 2, using TMA, SiH4, NH3 and N2O, a total of four special gases, to pass into the PECVD equipment to produce an aluminum-doped silicon oxynitride layer, the refractive index of the aluminum-doped silicon oxynitride layer is controlled between 1.4 and 1.8, and the thickness of the aluminum-doped silicon oxynitride layer is between 10 and 50 nm;
[0087] Step 3: On the surface of the aluminum-doped silicon oxynitride layer, a silicon oxynitride layer is deposited using three special gases, SiH4, NH3 and N2O, wherein the refractive index of the silicon oxynitride layer is between 1.6 and 1.9, and the thickness of the silicon oxynitride layer is controlled to be between 10 and 20 nm;
[0088] Step 4: On the surface of the silicon nitride oxide layer, a first silicon nitride layer is made by using two special gases, SiH4 and NH3, with a refractive index between 2.35 and 2.25, and a thickness of the first silicon nitride layer is controlled between 10 and 35 nm;
[0089] Step 5: On the surface of the first silicon nitride layer, a second silicon nitride layer is made by using two special gases, SiH4 and NH3, with a refractive index between 2.25 and 2.1, and a thickness of the second silicon nitride layer is controlled between 10 and 20 nm;
[0090] Step 6: On the surface of the second silicon nitride layer, use SiH4 and NH3 as two special gases to make a third silicon nitride layer with a refractive index between 2.1 and 1.9. The thickness of the third silicon nitride layer is controlled at 10 to 20 nm.
[0091] The present application also provides a battery back passivation structure, and the battery back passivation structure is manufactured by the battery back passivation structure manufacturing method as described in any of the above embodiments.
[0092] The battery back passivation structure in the present application includes a doped passivation layer and an internal reflection layer stacked on the back of a silicon wafer, and the passivation ability is enhanced; in the present application, when depositing the doped passivation layer, the doping gas and the first reaction gas are simultaneously introduced into the coating equipment for deposition, that is, the doped passivation layer is obtained by one step, avoiding the method of first depositing the passivation layer and then doping the passivation layer by diffusion or ion implantation, shortening the preparation time of the doped passivation layer, and avoiding the diffusion or ion implantation process causing damage to the passivation layer, thereby affecting the performance of the back passivation structure; since the deposited doped passivation layer has a strong passivation performance, the thickness of the doped passivation layer can be thinned, shortening the preparation process time, and thus reducing defects such as wrap-around plating / back field boat printing.
[0093] The present application also provides a solar cell, which includes the cell back passivation structure described in the above embodiment.
[0094] The solar cell may be a bifacial PERC (Passivated Emitter Rear Contact) cell, or a PERL (Passivated Emitter and Rear Locally-diffused) cell, and the like.
[0095] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0096] The above is a detailed introduction to a battery back passivation structure and its manufacturing method, and a solar cell provided by the present application. This article uses specific examples to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method and its core idea of the present application. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.
Claims
1. A method for manufacturing a battery back passivation structure, characterized in that: include: A doping gas and a first reaction gas are introduced into the coating device to deposit a doped passivation layer on the back side of the silicon wafer; the first reaction gas includes SiH4, NH3 and N2O, and the doped passivation layer is a doped silicon oxynitride layer; After depositing a doped passivation layer on the back of the silicon wafer, introducing the first reaction gas into the coating device to deposit a silicon oxynitride layer on the surface of the doped passivation layer away from the silicon wafer; the refractive index of the silicon oxynitride layer is greater than the refractive index of the doped silicon oxynitride layer; and the thickness of the silicon oxynitride layer is 10 to 20 nm; A second reaction gas is introduced into the coating device to deposit an internal reflection layer on the surface of the silicon oxynitride layer away from the doped passivation layer; the second reaction gas includes SiH4 and NH3, and the internal reflection layer is a silicon nitride layer; Depositing an internal reflection layer on a surface of the silicon oxynitride layer away from the doped passivation layer comprises: A plurality of internal reflection layers stacked in sequence are deposited on a surface of the silicon oxynitride layer away from the doped passivation layer.
2. The method for manufacturing a battery back passivation structure according to claim 1, characterized in that: The doping gas includes a gas containing phosphorus, boron, aluminum, gallium, and indium.
3. The method for manufacturing a battery back passivation structure according to claim 1, characterized in that: In a direction away from the silicon wafer, the refractive index of the multiple internal reflection layers stacked in sequence gradually decreases.
4. The method for manufacturing a battery back passivation structure according to claim 3, characterized in that: The number of layers of the internal reflection layer is three.
5. The method for manufacturing a battery back passivation structure according to claim 4, characterized in that: In the direction away from the silicon oxynitride layer, the refractive index of the first internal reflection layer is between 2.35 and 2.25, and the thickness is between 10nm and 35nm; the refractive index of the second internal reflection layer is between 2.25 and 2.1, and the thickness is between 10nm and 20nm; the refractive index of the third internal reflection layer is between 2.1 and 1.9, and the thickness is between 10nm and 20nm.
6. The method for manufacturing a battery back passivation structure according to any one of claims 1 to 5, characterized in that: The doping gas and the first reaction gas are introduced into the coating device, and before the doped passivation layer is deposited on the back side of the silicon wafer, the method further includes: The silicon wafer is subjected to acid polishing or alkaline polishing.
7. A battery back passivation structure, characterized in that: The battery back passivation structure is manufactured by the battery back passivation structure manufacturing method according to any one of claims 1 to 6.
8. A solar cell, characterized in that: The solar cell comprises the cell back passivation structure as claimed in claim 7.
Citation Information
Cited By
Battery back passivation structure, manufacturing method therefor, and solar cell
WO2023036121A1