Porous three-dimensional micro-pillar array material, preparation method and application thereof

Porous three-dimensional micro-pillar array materials are prepared through inkjet printing technology as a growth template for oxide semiconductor films, which solves the high cost and long cycle problems of preparing pillar gas sensors in the existing technology, and realizes efficient and low-cost gas sensors. Preparation, with higher gas response and shorter response recovery time.

CN114113242BActive Publication Date: 2024-10-29SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202111487647.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-07
Publication Date
2024-10-29
Estimated Expiration
2041-12-07

AI Technical Summary

Technical Problem

The existing methods for preparing column gas sensors are expensive, complex and have long manufacturing cycles, making it difficult to prepare efficient and low-cost porous three-dimensional micro-column array materials.

Method used

The nanomaterial dispersion is printed on a freezing platform using inkjet printing technology, and a porous three-dimensional micropillar array material is formed by freeze-drying, and an oxide semiconductor film is grown on it as a template, and a gold interdigital electrode is set to prepare a pillar gas. sensor.

Benefits of technology

The rapid preparation of porous three-dimensional micropillar array materials with high aspect ratio and large specific surface area is achieved, which reduces the process cost, shortens the manufacturing cycle, and improves the response speed and recovery time of the gas sensor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114113242B_ABST
    Figure CN114113242B_ABST
Patent Text Reader

Abstract

The present invention discloses a porous three-dimensional micro-column array material, a preparation method and application thereof. The preparation method comprises: using a nano-material dispersion as ink, and printing the ink on a substrate of a freezing platform by inkjet printing to form a nano-material micro-column array; then freeze-drying it to obtain a porous three-dimensional micro-column array material. The present invention prepares a porous three-dimensional micro-column array material with a high aspect ratio and a large specific surface area by combining inkjet printing with a freezing platform, without any support or mask, and with low process cost; the entire printing process can be completed within a few minutes, with a short manufacturing cycle and great application value; and the porous three-dimensional micro-column array prepared by the present invention can be used as a template for the growth of oxide semiconductor thin films, so as to prepare a columnar gas sensor, which can be used to monitor a variety of gases, and has a higher gas response, shorter response and recovery time than a planar sensor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for preparing a porous material, and in particular to a porous three-dimensional microcolumn array material used in a sensor and a preparation method thereof, as well as application in preparing a sensor, and belongs to the technical field of additive manufacturing. Background Art

[0002] Gas sensors for detecting various gases including toxic, flammable, organic, cooking vapors, etc. are in high demand in industrial, automotive, clinical, environmental monitoring, and household sectors. Among all these sensors, sensors based on metal oxide semiconductors such as ZnO, CdO, and SnO are one of the most widely studied chemiresistor gas sensors. 2 . The sensing mechanism of the gas sensor is based on the change of its conductivity in the presence of reducing and oxidizing gases. ZnO is used as an example to illustrate the principle. ZnO is a cheap, non-toxic, abundant n-type semiconductor with a wide direct band gap (3.37 eV) and high exciton energy (60 meV). It is one of the most promising metal oxide semiconductor materials. At certain temperatures, oxygen is adsorbed on the surface of ZnO in the form of O- ions, extracting electrons from the ZnO conduction band and producing a depletion layer, which leads to a decrease in the conductivity of the material; in the presence of reducing gases in the atmosphere, they react with O adsorbed on the surface of the ZnO crystal. -离 The O - The concentration of ions decreases, which increases the conductivity of ZnO. Since the response of chemical sensors depends on the surface reaction between the structure and gas molecules, the shape and size of the structure are key parameters of the sensing material. Currently, most mainstream gas sensors are planar. In contrast, columnar gas sensors have a large surface area ratio, which can increase the number of sensitive materials and gas absorption surfaces, thereby further improving the sensing performance of the sensor, with higher gas response, shorter response and recovery time than planar sensors. Therefore, improving the aspect ratio and specific surface area of ​​gas-sensitive materials is very meaningful for the application of gas sensors.

[0003] The current mainstream method for preparing columnar gas sensors is to use photolithography to obtain a microcolumn array, which is used as a template for the gas sensor to increase the specific surface area of ​​the sensing material, and then deposit a metal thin film ZnO on the surface of the microcolumns. In this preparation method, photolithography brings huge cost challenges to this method, and the complexity of the photolithography process also limits its practical application. Therefore, there is an urgent need to develop an efficient, low-cost, convenient and fast manufacturing method. Summary of the invention

[0004] The main purpose of the present invention is to provide a porous three-dimensional micro-column array material and a preparation method thereof, so as to overcome the deficiencies in the prior art.

[0005] Another object of the present invention is to provide the application of porous three-dimensional micro-column array material in the preparation of sensors.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0007] An embodiment of the present invention provides a method for preparing a porous three-dimensional micro-pillar array material, which comprises:

[0008] Providing nanomaterial dispersions;

[0009] Using the nanomaterial dispersion as ink, printing the ink on a substrate of a freezing platform in an inkjet printing manner to form a nanomaterial microcolumn array;

[0010] The nano material micro-column array is freeze-dried and molded to obtain a porous three-dimensional micro-column array material.

[0011] In some embodiments, the preparation method specifically comprises:

[0012] Using inkjet printing, the ejected ink droplets are sprayed onto the substrate of the freezing platform and quickly turned into a solid state, realizing material deposition in the vertical and horizontal directions, and stacking layer by layer to produce a three-dimensional nanomaterial microcolumn array structure.

[0013] The embodiment of the present invention also provides a porous three-dimensional micro-pillar array material prepared by the above method. The maximum aspect ratio of the porous three-dimensional micro-pillar array material reaches 12:1, and the porosity is 30% to 50%.

[0014] The embodiment of the present invention also provides the use of the porous three-dimensional micro-column array material in preparing a sensor.

[0015] The embodiment of the present invention further provides a method for preparing a column-type gas sensor, which comprises:

[0016] Using the porous three-dimensional micro-pillar array material as a growth template, magnetron sputtering grows an oxide semiconductor film on the porous three-dimensional micro-pillar array material;

[0017] And, a gold interdigital electrode is arranged on the oxide semiconductor film to obtain a columnar gas sensor.

[0018] The embodiment of the present invention also provides a column-type gas sensor prepared by the above method.

[0019] Furthermore, an embodiment of the present invention also provides application of the column-type gas sensor in the field of gas monitoring.

[0020] Compared with the prior art, the beneficial effects of the present invention are at least:

[0021] The present invention prepares a porous three-dimensional microcolumn array material with a high aspect ratio and a large specific surface area by combining inkjet printing with a freezing platform. No support or mask is required, and the process cost is low. The entire printing process can be completed within a few minutes, the manufacturing cycle is short, and it has great application value. In addition, the porous three-dimensional microcolumn array prepared by the present invention can be used as a template for the growth of oxide semiconductor films to prepare columnar gas sensors, which can be used to monitor a variety of gases and have higher gas response and shorter response and recovery time than planar sensors. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 is a schematic diagram of the preparation process of a column-type gas sensor in a typical embodiment of the present invention;

[0024] Figure 2 It is a flow chart of preparing a column-type gas sensor in a typical embodiment of the present invention. DETAILED DESCRIPTION

[0025] In view of the disadvantages of existing traditional methods such as high cost, complex process and long manufacturing cycle, the inventor of this case, after long-term research and extensive practice, was able to propose the technical solution of the present invention, which is mainly to quickly and low-cost prepare columnar gas sensors.

[0026] Conventional inkjet printing is difficult to print a true three-dimensional structure without auxiliary means. The present invention uses an inkjet printing structure and a freezing platform to prepare a porous microcolumn array with a high aspect ratio and a large specific surface area without any support or mask.

[0027] The technical solution, its implementation process and principle will be further explained as follows.

[0028] One aspect of an embodiment of the present invention provides a method for preparing a porous three-dimensional micro-pillar array material, comprising:

[0029] Providing nanomaterial dispersions;

[0030] Using the nanomaterial dispersion as ink, printing the ink on a substrate of a freezing platform in an inkjet printing manner to form a nanomaterial microcolumn array;

[0031] The nano material micro-column array is freeze-dried and molded to obtain a porous three-dimensional micro-column array material.

[0032] In some embodiments, the nanomaterial dispersion includes nanomaterial and a solvent.

[0033] In some embodiments, the nanomaterial may be silicon dioxide, or any one or a combination of two or more nanomaterials such as polystyrene and titanium dioxide, but is not limited thereto.

[0034] Furthermore, the particle size of the silicon dioxide is 20 to 100 nm, the particle size of the polystyrene is 150 to 300 nm, and the particle size of the titanium dioxide is 10 to 30 nm.

[0035] Furthermore, the concentration of the nanomaterial in the nanomaterial dispersion is 60-75 mg / mL.

[0036] Furthermore, the solvent is a mixture of water, tert-butyl alcohol and propylene glycol.

[0037] In some embodiments, the nanomaterial microcolumn array is composed of a plurality of microcolumn structures, the nanomaterial microcolumns have a diameter of 60 to 100 μm, a height of 400 to 700 μm, and a spacing between adjacent nanomaterial microcolumns of 100 to 130 μm.

[0038] In some embodiments, the process parameters of the inkjet printing include: a voltage of 25 to 30 V, a frequency of 1 to 2 kHz, and a nozzle diameter of 20 μm.

[0039] In some embodiments, the preparation method specifically comprises:

[0040] Using inkjet printing, the ejected ink droplets are sprayed onto the substrate of the freezing platform and quickly turned into a solid state, realizing material deposition in the "Z direction" (where the "Z" direction indicates the vertical horizontal direction, which is the opposite direction of gravity), and stacking layers to form a three-dimensional silica microcolumn array structure.

[0041] In some embodiments, the freeze-drying temperature is -70°C to -40°C, and the time is 18 to 24 hours.

[0042] The present invention utilizes inkjet printing combined with a freezing platform. The principle is that ink droplets are sprayed onto a freezing platform substrate and quickly become solid, fixing the shape of the ink droplets, realizing material deposition in the "Z direction", and preparing a three-dimensional microcolumn structure by stacking layer by layer. After freeze-drying, the structure is directly formed without any support or mask, and the process cost is low. The entire printing process can be completed within a few minutes, with a short manufacturing cycle and great application value. This method can prepare porous microcolumn arrays with a high aspect ratio and a large specific surface area, has the advantages of low cost and a short manufacturing cycle, and in theory any material that can be frozen can be realized, and a method for preparing a three-dimensional microcolumn array by inkjet printing is clarified.

[0043] Another aspect of the embodiments of the present invention further provides a porous three-dimensional micro-pillar array material prepared by the aforementioned method.

[0044] Furthermore, the maximum aspect ratio of the porous three-dimensional micro-pillar array material reaches 12:1, and the porosity is 30% to 50%.

[0045] Another aspect of the embodiments of the present invention further provides the use of the porous three-dimensional micro-pillar array material in preparing a sensor.

[0046] Another aspect of the embodiments of the present invention further provides a method for preparing a columnar gas sensor, which comprises:

[0047] Using the porous three-dimensional micro-pillar array material as a growth template, magnetron sputtering grows an oxide semiconductor film on the porous three-dimensional micro-pillar array material;

[0048] And, a gold interdigital electrode is arranged on the oxide semiconductor film to obtain a columnar gas sensor.

[0049] Wherein, the thickness of the oxide semiconductor film is 150nm to 500nm.

[0050] In some specific embodiments, see Figure 1 As shown, the preparation method of the column type gas sensor is mainly divided into two parts, specifically including:

[0051] 1) Using silica dispersion as ink, the ink is printed through a nozzle on a -70°C to -40°C freezing platform by inkjet printing, and then freeze-dried to obtain a silica porous three-dimensional microcolumn array template (i.e., the "silica microcolumn array" in the figure).

[0052] 2) Magnetron sputtering deposition of metal oxide semiconductor films and gold interdigitated electrodes.

[0053] Another aspect of the embodiments of the present invention further provides a column-type gas sensor prepared by the aforementioned method.

[0054] The present invention uses the porous three-dimensional micro-column array with high aspect ratio and large specific surface area prepared above as a template for the growth of oxide semiconductor film to prepare a columnar gas sensor, which has higher gas response and shorter response and recovery time than a planar sensor.

[0055] For example, for a planar gas sensor, the average response time is 67 seconds, and the average recovery time is 165 seconds, while the average response time of the columnar gas sensor prepared by the present invention is 64 seconds, and the average recovery time is 124 seconds.

[0056] Correspondingly, another aspect of the embodiments of the present invention further provides application of the column-type gas sensor in the field of gas monitoring.

[0057] The gas may be ethanol, acetone, etc., but is not limited thereto.

[0058] In a more specific implementation example provided by the present invention, the flow chart of the column type gas sensor is as follows Figure 2 The whole process includes:

[0059] (1) Preparation of silica dispersion

[0060] (2) Surface tension and viscosity test of silica dispersion

[0061] (3) Debug inkjet printer parameters (voltage, frequency, etc.)

[0062] (4) Printing of silica micropillar arrays on frozen substrates (with ice crystals before drying)

[0063] (5) Freeze drying to obtain porous three-dimensional silica microcolumn arrays

[0064] (6) Magnetron sputtering growth of oxide semiconductor films and gold interdigitated electrodes

[0065] (7) Gas sensor performance test.

[0066] In summary, the present invention uses the printed porous micro-column array as a template for the growth of an oxide semiconductor film to prepare a columnar gas sensor, which can be used to monitor a variety of gases, such as ethanol, acetone, etc.

[0067] The present invention will be more fully understood through the following detailed description, which should be read in conjunction with the accompanying drawings. Detailed embodiments of the present invention are disclosed herein; however, it should be understood that the disclosed embodiments are only exemplary of the present invention, which can be embodied in various forms. Therefore, the specific functional details disclosed herein should not be interpreted as limiting, but only as the basis of the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in virtually any appropriate detailed embodiment.

[0068] Example 1

[0069] Prepare a silica dispersion with a concentration of 75 mg / mL, the solvent used is a mixture of water, tert-butyl alcohol and propylene glycol, and then load it into the ink cartridge. Set the various parameters of the printer, including the voltage of 30V, the frequency of 1kHz, the microcolumn diameter of 100μm, and the spacing of 100μm. After printing on the freezing platform 10-15 times, silica microcolumns of different heights (400-700μm in height) will appear. Then put it into a -40℃ freeze drying oven and vacuum dry it for 24 hours to obtain a porous silica microcolumn array. After preparing the microcolumns, use a ZnO ceramic target to deposit ZnO thin film in RF magnetron sputtering. Chamber bottom pressure ≤1×10 -4 Pa, the substrate temperature is room temperature, the working pressure is 1Pa, and the RF power is 100W. The deposition time is 30 minutes, and the thickness of the ZnO film is 150nm, which can be adjusted by the deposition time. Finally, Ti / Au interdigital electrodes are deposited on the surface of the ZnO film by magnetron sputtering, with Ti being 40nm and Au being 500nm, to obtain a columnar gas sensor.

[0070] Example 2

[0071] Prepare a polystyrene dispersion with a concentration of 65 mg / mL, the solvent used is a mixture of three solvents: water, tert-butyl alcohol and propylene glycol, and then load it into the ink cartridge. Set the various parameters of the printer, including the voltage of 25V, the frequency of 1.5kHz, the microcolumn diameter of 80μm, and the spacing of 120μm. After printing on the freezing platform 10-15 times, polystyrene microcolumns of different heights (400-700μm in height) will appear. Then put it into a -70℃ freeze drying oven and vacuum dry it for 18h to obtain a porous polystyrene microcolumn array. After preparing the microcolumns, use a ZnO ceramic target to deposit ZnO thin film in RF magnetron sputtering. Chamber bottom pressure ≤1×10 -4 Pa, the substrate temperature is room temperature, the working pressure is 1Pa, and the RF power is 100W. The deposition time is 30 minutes, and the thickness of the ZnO film is 350nm, which can be adjusted by the deposition time. Finally, Ti / Au interdigital electrodes are deposited on the surface of the ZnO film by magnetron sputtering, with Ti being 40nm and Au being 500nm, to obtain a columnar gas sensor.

[0072] Example 3

[0073] Prepare a titanium dioxide dispersion with a concentration of 60 mg / mL, the solvent used is a mixture of three solvents: water, tert-butyl alcohol and propylene glycol, and then load it into the ink cartridge. Set the various parameters of the printer, including the voltage of 28V, the frequency of 2kHz, the microcolumn diameter of 60μm, and the spacing of 130μm. After printing 10-15 times on the freezing platform, titanium dioxide microcolumns of different heights (400-700μm in height) will appear. Then put it into a -60℃ freeze drying oven and vacuum dry it for 20 hours to obtain a porous titanium dioxide microcolumn array. After preparing the microcolumns, use a ZnO ceramic target to deposit ZnO thin film in radio frequency magnetron sputtering. Chamber bottom pressure ≤1×10 -4 Pa, the substrate temperature is room temperature, the working pressure is 1Pa, and the RF power is 100W. The deposition time is 30 minutes, and the thickness of the ZnO film is 500nm, which can be adjusted by the deposition time. Finally, Ti / Au interdigital electrodes are deposited on the surface of the ZnO film by magnetron sputtering, with Ti being 40nm and Au being 500nm, to obtain a columnar gas sensor.

[0074] It has been detected that the columnar gas sensors obtained in the above Examples 1-3 can be used to monitor a variety of gases, such as ethanol, acetone, etc., and have higher gas response, shorter response and recovery time than planar sensors.

[0075] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made without departing from the spirit and scope of the present invention and that the elements of the embodiments may be replaced by substantial equivalents. In addition, many modifications may be made without departing from the scope of the present invention to adapt specific circumstances or materials to the teachings of the present invention. Therefore, it is not intended herein to limit the present invention to the disclosed specific embodiments for performing the present invention, but it is intended that the present invention will include all embodiments within the scope of the appended claims. In addition, unless specifically stated, any use of the terms first, second, etc. does not indicate any order or importance, but rather uses the terms first, second, etc. to distinguish one element from another.

Claims

1. A method for preparing a porous three-dimensional microcolumn array material, characterized in that: include: A nanomaterial dispersion is provided, wherein the nanomaterial dispersion comprises a nanomaterial and a solvent, wherein the nanomaterial is selected from any one of silicon dioxide, polystyrene, and titanium dioxide or a combination of two or more thereof, wherein the solvent is a mixture of water, tert-butyl alcohol, and glycerol, and wherein the concentration of the nanomaterial in the nanomaterial dispersion is 60-75 mg / mL; The nanomaterial dispersion is used as ink, and the ink droplets are ejected onto a substrate of a freezing platform in an inkjet printing manner to quickly become solid, thereby realizing material deposition in the vertical and horizontal directions, and stacking and forming a three-dimensional nanomaterial microcolumn array layer by layer. The process parameters of the inkjet printing include: a voltage of 25-30 V, a frequency of 1-2 kHz, a nozzle diameter of 20 µm, a diameter of the nanomaterial microcolumns in the nanomaterial microcolumn array of 60-100 µm, a height of 400-700 µm, and a spacing of 100-130 µm between adjacent nanomaterial microcolumns; The nano material micro-column array is freeze-dried and molded to obtain a porous three-dimensional micro-column array material.

2. The preparation method according to claim 1, characterized in that: The particle size of the silicon dioxide is 20-100 nm, the particle size of the polystyrene is 150-300 nm, and the particle size of the titanium dioxide is 10-30 nm.

3. The preparation method according to claim 1, characterized in that: The freeze-drying temperature is -70°C to -40°C, and the time is 18 to 24 hours.

4. A porous three-dimensional micropillar array material prepared by the preparation method according to any one of claims 1 to 3, wherein the porous three-dimensional micropillar array material has a maximum aspect ratio of 12:1 and a porosity of 30% to 50%.

5. Use of the porous three-dimensional microcolumn array material according to claim 4 in preparing a sensor.

6. A method for preparing a columnar gas sensor, characterized in that: include: Using the porous three-dimensional micro-pillar array material according to claim 4 as a growth template, magnetron sputtering grows an oxide semiconductor film on the porous three-dimensional micro-pillar array material; And, a gold interdigital electrode is arranged on the oxide semiconductor film to obtain a columnar gas sensor.

7. The preparation method according to claim 6, characterized in that: The thickness of the oxide semiconductor film is 150nm~500nm.

8. A columnar gas sensor prepared by the preparation method according to claim 6 or 7.

9. Application of the column-type gas sensor according to claim 8 in the field of gas monitoring.

10. The use according to claim 9, characterized in that: The gas is ethanol or acetone.

Citation Information

Patent Citations

  • Medical anti-sticking membrane and preparation method thereof

    CN101623517A

  • Post-treatment method for improving printing evenness of electronic material

    CN102529479A

  • Large-scale ink-jet printing method for three-dimensional metamaterial array

    CN106904002A

  • Organic field-effect transistor memory based on nano lattice molecules and preparation method thereof

    CN109524546A

  • Semiconductor gas sensor and preparation method thereof

    CN110057869A