A production process of PTFE high-frequency board

By adding auxiliary boards and multiple copper plating and flash plating processes to the PTFE high-frequency board production process, the problems of drilling and milling burrs and hole wall metallization are solved, and high-quality production efficiency and standard-compliant products are achieved.

CN114245589BActive Publication Date: 2024-10-15无锡市同步电子科技股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111625549.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-28
Publication Date
2024-10-15
Estimated Expiration
2041-12-28

AI Technical Summary

Technical Problem

The existing production process of PTFE high-frequency plates is prone to problems such as excessive drilling and milling burrs and difficulty in metallizing the hole walls, making it difficult to meet product acceptance standards and user requirements.

Method used

Adopting a simplified production process, including adding an auxiliary board before drilling, setting appropriate drilling parameters, performing plasma activation and multiple copper deposition and flash plating treatments to ensure hole wall integrity and metallization quality, and using sandwich plates The frame undergoes electroplating and pattern plating, through-hole thermal stress testing is performed, and finally segmented baking plate curing is performed.

Benefits of technology

It effectively reduces drilling and milling burrs, ensures the quality and integrity of hole wall metallization, improves the production efficiency and quality of PTFE high-frequency plates, and meets the acceptance requirements of existing standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003438651210000041
    Figure BDA0003438651210000041
  • Figure BDA0003438651210000051
    Figure BDA0003438651210000051
  • Figure BDA0003438651210000061
    Figure BDA0003438651210000061
Patent Text Reader

Abstract

The present invention discloses a production process of a PTFE high-frequency board and its application, and relates to the technical field of printed circuit board production and manufacturing. The steps of the production process of the PTFE high-frequency board disclosed in the present invention are: S1 cutting; S2 drilling; S3 plasma activation; S4 copper plating and flash plating; S5 electroplating and quality inspection; S6 outer layer pretreatment; S7 pattern plating and quality inspection; S8 outer layer alkaline etching and through-hole thermal stress test; S9 solder mask; S10 character, surface treatment, quality inspection, final inspection and packaging. The present invention provides a production process of a PTFE high-frequency board, which has a simple process flow and single parameters, and can reduce the problems of many drilling and milling burrs, difficulty in hole wall metallization, etc., while ensuring the final product acceptance standards and user requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of printed circuit board production and manufacturing, and in particular relates to a production process of a PTFE high-frequency board. Background Art

[0002] There are many types of high-frequency boards. Different material compositions have different requirements for the processing of printed circuit boards, especially for high-frequency board materials containing PTFE. There are special requirements for production equipment, processes and process parameters, which are mainly limited by the characteristics of PTFE materials. Otherwise, it is easy to have defects such as many drilling and milling burrs and difficulty in hole wall metallization. Summary of the invention

[0003] The main purpose of the present invention is to provide a production process for a PTFE high-frequency plate, which has a simple process flow and single parameters, and can reduce problems such as many drilling and milling burrs and difficulty in hole wall metallization, while ensuring the final product acceptance standards and user requirements.

[0004] In order to achieve the purpose of the present invention, the present invention provides a production process of a PTFE high-frequency plate, which specifically comprises the following steps:

[0005] S1. Cut the material and ensure the core board is flat, mark the board corners to avoid mixing with other core boards;

[0006] S2. Drilling: Drill the core material according to the set drilling parameters. The total thickness of the core material plus the thickness of the cover plate and the backing plate shall not exceed the length of the drill groove. Use an air gun to blow after drilling, and do not grind the plate;

[0007] S3. Plasma activation, activation parameters: N2: H2 = 600: 1400, power 7000W, activation time 70min, after activation, the dyne value is greater than 40 by using a dyne pen test;

[0008] S4. Copper plating and flash plating:

[0009] Copper deposition is carried out within 8 hours after plasma activation. Copper deposition 1 (i.e. the first copper deposition) starts from the high-position neutralization tank, and copper deposition 2 (i.e. the second copper deposition) starts from the prepreg tank to ensure the quality of copper deposition, without black holes and bubbles in the holes.

[0010] The copper plating and flash plating process is as follows:

[0011] 1) Before copper deposition, the thin plate rack should be installed first. Swinging during copper deposition will cause the plate to deform, and eventually lead to uncontrollable dimensional deformation.

[0012] 2) Copper deposition 1: After activation, copper deposition 1 is carried out, and cleaning is carried out in the same way as for multilayer boards, but potassium permanganate is not used. Conventional first copper deposition ensures flash plating after copper deposition on the hole wall.

[0013] 3) Flash plating: The main function is to thicken the hole wall copper, and the flash plating parameters are set to 1.0asd / 30min.

[0014] 4) Copper deposition 2: Since the copper deposition effect of PTFE material is poor, in order to avoid star-point voids in the hole wall after one copper deposition, copper deposition is performed again after flash plating to ensure the integrity of the hole wall.

[0015] S5. Clamp the thin plate frame for electroplating, clamp the long side, make the copper thickness of the electroplated hole greater than 13μm, and the surface copper thickness greater than 18μm, and then check the electroplated copper thickness and drilling quality;

[0016] S6. Use conventional methods to pre-treat the outer layer, and the pre-treatment should not be excessively abrasive or brushed;

[0017] S7. Clamp the thin plate frame for pattern plating, clamp the long side, make the copper thickness of the pattern plated hole>28μm, then check the copper plating thickness of the pattern, make the surface copper thickness>43μm;

[0018] S8. After adding the outer layer with the board, alkali etching is performed, and then the through-hole thermal stress test is performed to ensure that the hole wall copper and the hole wall meet the quality inspection requirements;

[0019] S9. Solder mask: Use the inner layer mode to treat the board surface dirt and increase the roughness through the circuit pre-processing line, and then do solder mask after entering the clean room. The solder mask ink is printed by spray printing. After the spray printing is completed, pre-curing is completed within 4 hours, and then solder mask testing is carried out, and then post-curing is carried out;

[0020] S10. Use conventional methods to control characters, conventional surface treatment, and then conduct conventional quality inspection, final inspection and packaging.

[0021] Furthermore, in step S2, an auxiliary plate needs to be added to the core board (i.e., substrate or core board material) before drilling, and the auxiliary plate and the substrate are composed of: aluminum sheet, copper substrate, substrate, copper substrate, phenolic base plate from top to bottom; when the hole diameter of the drilled hole is greater than 0.6 mm, a 0.4 mm phenolic cover plate is added to the aluminum sheet.

[0022] The substrate is a PTFE high-frequency board that needs to be processed. The copper substrate refers to an auxiliary board used for protection and reducing drilling burrs. The aluminum sheet is used for drilling buffer positioning and heat dissipation. From the perspective of the comprehensive concept of PTFE material: cover plate = aluminum sheet + copper substrate, pad plate = phenolic base plate + copper substrate. The phenolic base plate (i.e. pad plate) also plays a role in protecting and reducing burrs. It has a high hardness and can effectively remove PTFE drill chips on the blade. When the aperture of the drill hole is larger, that is, the aperture is greater than 0.6mm, more drill chips are generated, and a 0.4mm phenolic cover plate needs to be added to the aluminum sheet.

[0023] Furthermore, the substrate is composed of PTFE and glass fiber.

[0024] Furthermore, the drilling parameters in step S2 are set as follows: needle diameter is 0.15-3.2 mm, rotation speed is 110-40 Krpm, feed speed is 1.0-3.3 m / min, and retract speed is 12-25 m / min.

[0025] Furthermore, after drilling in step S2, the copper surface is treated by an inner layer circuit pre-treatment line and then baked at 120° C. for 1 hour.

[0026] Furthermore, in the step S10, the printing is thin plate printing, and the thin plate printing is performed by two single-sided printing and single-sided pre-baking.

[0027] Furthermore, in step S10, the post-curing adopts a segmented baking method, and its parameters are set as follows: the temperature of the first section is 70°C, and the baking time is 60 minutes; the temperature of the second section is 90°C, and the baking time is 60 minutes; the temperature of the third section is 110°C, and the baking time is 30 minutes; the temperature of the fourth section is 130°C, and the baking time is 30 minutes; the temperature of the fifth section is 150°C, and the baking time is 60 minutes.

[0028] The present invention has achieved the following beneficial effects:

[0029] 1. The PTFE high-frequency board of the present invention has a simple production process and single parameters, which is convenient for production operation. It has been verified that the effects of the PTFE high-frequency board can pass various tests and meet existing standards.

[0030] 2. The present invention uses debugged drilling parameters (such as rotation speed, feed speed, retract speed, etc.) and drilling methods (adding auxiliary plates and thickness settings, etc.) to reduce the problem of many burrs in drilling and milling; uses plasma activation to remove glue, and adds a flash plating process after hole activation to solve the problem of difficult hole wall metallization, making subsequent hole processing convenient and improving the production efficiency and quality of PTFE high-frequency plates. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] The production process of the PTFE high-frequency board of the present invention is described below in conjunction with specific embodiments.

[0033] The present invention provides a specific production process of a PTFE high-frequency board in combination with actual production, as follows.

[0034] 1. Test board preparation

[0035] According to the processing requirements, the production board is prepared with a thickness of 0.254mm, a copper thickness of 18 / 18, and a size of 9*12inch.

[0036] 2. The processing flow of PTFE high-frequency board includes the following steps:

[0037] S1. Cutting:

[0038] 1. The core board (i.e. core board material) is flat after cutting;

[0039] 2. Mark the board corners to avoid mixing with other core boards.

[0040] S2. Drilling:

[0041] 1. Drill according to the drilling parameters. The drilling parameters are set as follows: needle diameter is 0.15-3.2mm, rotation speed is 110-40Krpm, feed speed is 1.0-3.3m / min, and retract speed is 12-25m / min. The specific values ​​are shown in the following table;

[0042]

[0043]

[0044]

[0045] 2. Before drilling, auxiliary plates need to be added to the upper and lower bottom surfaces of the core board material. The stacking structure of the core board material and the auxiliary plates from bottom to top is: 1.5mm phenolic base plate + 0.15mm copper substrate + base plate (i.e. core board material) + 0.15mm copper substrate + aluminum sheet. When the hole diameter is greater than 0.6mm, a 0.4mm phenolic cover plate is added to the aluminum sheet. The total thickness of the core board material plus the cover plate (i.e. 0.15mm copper substrate + aluminum sheet) and the pad (i.e. 1.5mm phenolic base plate + 0.15mm copper substrate) shall not exceed the length of the drill groove;

[0046] 3. Use an air gun to blow after drilling, do not grind the board, and process the copper surface through the inner layer circuit pre-processing line;

[0047] 4. Bake at 120℃ for 1h after drilling.

[0048] S3. Plasma activation:

[0049] 1. Activation parameters: N2:H2=600:1400, power: 7000W, activation time: 70min;

[0050] 2. After activation, the dyne value is greater than 40 when tested with a dyne pen;

[0051] 3. After activation, copper is deposited within 8 hours.

[0052] S4. Copper deposition 1:

[0053] Before copper deposition, it is necessary to install the thin plate rack first. Swinging during copper deposition will cause the plate to deform, and eventually lead to uncontrollable dimensional deformation. After activation, copper deposition 1 (first copper deposition) is cleaned in the same way as multilayer boards, but potassium permanganate is not used. The conventional first copper deposition starts from the high-position neutralization tank to ensure flash plating after copper deposition on the hole wall. Copper deposition must be carried out within 8 hours after plasma activation.

[0054] S5. Flash plating: Flash plating is completed within 4 hours after copper deposition 1 is completed. The main function is to thicken the hole wall copper. The flash plating parameter is set to 1.0asd / 30min. The thin plate frame also needs to be clamped during flash plating.

[0055] S6. Copper deposition 2: Since the copper deposition effect of PTFE material is poor, in order to avoid star-point voids in the hole wall after one copper deposition, copper deposition is performed again after flash plating, starting from the prepreg tank to ensure the integrity of the hole wall and the quality of copper deposition, without black holes and bubbles in the holes.

[0056] S7. Electroplating:

[0057] 1. The copper thickness of the electroplated hole is greater than 13μm, and the long side is clamped;

[0058] 2. Clamp the thin plate frame during electroplating;

[0059] 3. Check the thickness of electroplated copper: electroplated hole copper>13μm, surface copper>18μm;

[0060] 4. Drilling quality inspection: After electroplating, take a slice to observe the parameters in the test hole, and there should be no wicking and rough hole wall problems.

[0061] S8. Outer layer: Use conventional methods for pre-treatment, and do not over-grind or over-brush.

[0062] S9. Image plating:

[0063] 1. The plated hole copper is greater than 28μm, and the long side is clamped;

[0064] 2. Clamp the thin plate frame during plating.

[0065] 3. Check the copper plating thickness: hole copper>28μm, surface copper>43μm.

[0066] S10. Alkali corrosion of outer layer:

[0067] 1. Add a strip during alkaline etching and apply solder resist ink within 8 hours after alkaline etching;

[0068] 2. Via thermal stress test: Take 3 slices of 15*8mm with a 0.5mm aperture, and test them under 288℃ / 10S test conditions, and tin-bleaching test 3 times / 5 times / 10 times, and observe after filling with glue: whether the copper on the hole wall is separated from the hole wall.

[0069] S11.Solder mask:

[0070] 1. The material is special, and the solder mask pre-treatment cannot be excessively brushed or sandblasted. The inner layer mode can be used to treat the board surface dirt and increase the roughness through the circuit pre-treatment line. After entering the clean room, solder mask is done, and the ink is sprayed within 8 hours after the outer layer graphics are completed;

[0071] 2. The solder mask ink is printed by spray printing, and the thin plate printing adopts the method of double single-sided printing and single-sided pre-baking;

[0072] 3. Pre-curing should be completed within 4 hours after printing is completed;

[0073] 4. Post-curing must be carried out in sections, parameters: 70℃ / 60min→90℃ / 60min→110℃ / 30min→130℃ / 30min→150℃ / 60min;

[0074] 5. Check the solder mask for problems such as misalignment before post-curing.

[0075] S12. Use conventional methods to control characters, conventional surface treatment, and then conduct conventional quality inspection, final inspection and packaging. During the routine quality inspection, ensure that the core board material has no scratches, pits, oxidation and gaps.

[0076] After the above PTFE high frequency board is completed, the test items are as follows:

[0077] 1. Test results of substrate material properties

[0078]

[0079] Test results: The test results of substrate material properties meet the standards

[0080] 2. Drilling hole wall quality test results

[0081]

[0082] Test results: The test results of the drilling hole wall quality meet the standards

[0083] 3. Porous electroplating quality inspection results

[0084]

[0085] Test results: The quality inspection results of hole plating are qualified

[0086] 4. Surface and electrical performance test results

[0087]

[0088] Test results: Appearance and electrical performance results are qualified

[0089] From the above verification results, it can be seen that the expected effect can be met.

[0090] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0091] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A production process of PTFE high-frequency board, characterized in that: The specific steps include: S1. Cut the material and ensure the core board is flat, and mark the board corners; S2. Drilling: Drill the core material according to the set drilling parameters. The total thickness of the core material plus the thickness of the cover plate and the backing plate shall not exceed the length of the drill groove. S3. Plasma activation, activation parameters: N2: H2 = 600: 1400, power 7000W, activation time 70min, after activation, the dyne value is greater than 40 by using a dyne pen test; S4. Copper deposition and flash plating: first install the thin plate rack, and then perform the first copper deposition after plasma activation. Clean it in the same way as the multilayer board, but use potassium permanganate, conventional copper deposition, and start from the high-position neutralization tank; flash plating, the flash plating parameters are set to 1.0asd / 30min; perform the second copper deposition, and start from the pre-preg tank; S5. Clamp the thin plate frame for electroplating, clamp the long side, make the copper thickness of the electroplated hole >13μm, and then check the electroplated copper thickness and drilling quality; S6. Use conventional methods to pre-treat the outer layer, and do not over-grind or brush; S7. Clamp the thin plate frame for pattern plating, clamp the long side, make the copper thickness of the pattern plated hole>28μm, then check the copper plating thickness of the pattern, make the surface copper thickness>43μm; S8. After adding the outer layer with the board, alkali etching is performed, and then the through-hole thermal stress test is performed to ensure that the hole wall copper and the hole wall meet the quality inspection requirements; S9. Solder mask: Use the inner layer mode to treat the board surface dirt and increase the roughness through the circuit pre-processing line. After entering the clean room, solder mask is applied. The solder mask ink is printed by spray printing. After the spray printing is completed, pre-curing is completed within 4 hours. Then solder mask detection is carried out, and then post-curing is carried out. S10. Routine control characters, surface treatment, quality inspection, final inspection, and packaging; In the step S2, before drilling the core board, an auxiliary board needs to be added, and the auxiliary board and the base board are composed of: aluminum sheet, copper substrate, base board, copper substrate, phenolic base board from top to bottom; when the hole diameter of the drilled hole is greater than 0.6 mm, a 0.4 mm phenolic cover board is added to the aluminum sheet; The substrate is composed of PTFE and glass fiber; The drilling parameters in step S2 are set as follows: needle diameter is 0.15-3.2 mm, rotation speed is 110-40 Krpm, feed speed is 1.0-3.3 m / min, and retract speed is 12-25 m / min; After drilling in step S2, the copper surface is treated by the inner layer circuit pre-treatment line and then baked at 120° C. for 1 hour; In the step S9, the printing is thin plate printing, and the thin plate printing is performed by two single-sided printing and single-sided pre-baking methods; In step S9, the post-curing adopts a segmented baking method, and its parameters are set as follows: the temperature of the first section is 70°C, and the baking time is 60 minutes; the temperature of the second section is 90°C, and the baking time is 60 minutes; the temperature of the third section is 110°C, and the baking time is 30 minutes; the temperature of the fourth section is 130°C, and the baking time is 30 minutes; the temperature of the fifth section is 150°C, and the baking time is 60 minutes.