A method for detecting NO2 using a semiconductor sensor and a method for preparing a composite metal oxide
By using the composite metal oxide ZnO-NiCo2O4 to construct a p-n heterojunction semiconductor sensor, the problem of insufficient selectivity and response ability of the sensor at low temperatures in the existing technology is solved, and high-sensitivity detection of NO2 gas is achieved, and it can be used in multiple applications. Maintain good detection results in the presence of various interfering gases.
Patent Information
- Application Number
- CN202011452656.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-12-12
AI Technical Summary
Existing semiconductor metal oxide sensors work at high temperatures, have poor selectivity, poor response and recovery capabilities, are difficult to effectively detect trace amounts of NO2 gas in low temperature environments, and are easily interfered by volatile organic compounds.
The composite metal oxide ZnO-NiCo2O4 is used as the sensing material, and microspheres with macroporous and mesoporous structures are prepared through hydrothermal reaction to construct a p-n heterojunction. The sensor is prepared by combining a simple drop coating method, and is heated at 50-300°C. Conduct resistance change testing within a temperature range to eliminate interfering gases and improve detection sensitivity and selectivity.
It achieves high selectivity and high sensitivity detection of NO2 gas at lower temperatures, has good response and recovery performance, can accurately detect trace amounts of NO2 in the presence of a variety of interfering gases, and has a simple process and good processability.
Smart Images

Figure HDA0002832243840000011 
Figure HDA0002832243840000012 
Figure HDA0002832243840000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of quantitative analysis methods of nano materials, and specifically relates to a method for detecting NO2 with a semiconductor sensor and a method for preparing a composite metal oxide ZnO-NiCo2O4. Background Art
[0002] In recent years, air pollution has seriously endangered people's health and has attracted widespread attention. Among them, nitrogen dioxide (NO2) is one of the gases that is most harmful to the human body. A concentration of 1ppm of NO2 will irritate the nose, eyes, and throat. A concentration of 50ppm of NO2 will cause abnormal breathing within one minute, and more than 200ppm can cause instant death. Long-term exposure to a certain concentration of NO2 will increase the chance of respiratory infections and lung diseases. In addition, NO2 is one of the causes of acid rain and photochemical smog, which is extremely harmful to the environment. Therefore, it is very necessary to develop sensors with real-time, sensitive, and rapid NO2 detection functions to ensure the safety of the public and humans.
[0003] With the advantages of cheap and abundant raw materials, green and environmentally friendly, convenient preparation, and simple operation, metal oxide semiconductor sensors have developed rapidly in recent years and attracted the attention of researchers. Common semiconductor metal oxides can be divided into simple oxides such as ZnO, NiO, In2O3, WO3 and composite metal oxides such as NiCo2O4, ZnCo2O4, etc. However, at present, most semiconductor metal oxide sensors still fail to overcome the shortcomings of high operating temperature (above 150°C), weak selectivity, poor response and recovery ability. Researchers often use methods such as doping precious metal elements, preparing composite metal oxides, constructing pn heterojunctions, designing porous and morphological methods to improve the sensing performance of semiconductor sensors. The present invention uses composite metal oxide ZnO-NiCo2O4 as a material for NO2 sensing. The presence of surface mesopores and the construction of pn heterojunctions enable this sensor to achieve a relatively low temperature NO2 (100°C) sensing effect, good stability and obvious selectivity, which is of great significance to the further development of semiconductor metal oxides. Summary of the invention
[0004] The purpose of the present invention is to provide a method for detecting NO2 using a semiconductor sensor, which can eliminate the interference of common inorganic gases and volatile organic compounds, has high selectivity and high sensitivity under a relatively low temperature working environment, and has good response recovery and repeatability, and can meet the detection needs of trace NO2 in actual environments.
[0005] On the one hand, the present invention provides a method for detecting NO2 using a semiconductor sensor, using a composite metal oxide ZnO-NiCo2O4 as a sensing film of the semiconductor sensor;
[0006] Preferably, the composite metal oxide ZnO-NiCo2O4 has macropores and mesopores, and the microscopic morphology is microspheres with an average particle size of 400-500 nm.
[0007] On the other hand, the present invention provides a method for preparing a composite metal oxide ZnO-NiCo2O4, wherein the raw materials comprising a nickel source and a cobalt source are subjected to a hydrothermal reaction, hydrolyzed in a zinc salt solution, and finally calcined to obtain the composite metal oxide.
[0008] Preferably, the method comprises the following steps: subjecting a nickel source, a cobalt source and glycerol to a hydrothermal reaction to obtain bimetallic glycerol nanospheres, subjecting the nanospheres to a hydrolysis reaction in a zinc nitrate solution, and finally calcining to obtain a composite metal oxide.
[0009] On the other hand, the present invention provides a method for preparing a semiconductor sensor, comprising the following steps: dispersing the composite metal oxide ZnO-NiCo2O4 in a solvent to make it uniformly dispersed, using a pipette to transfer the uniformly dispersed suspension to prepare a film, and arranging parallel electrodes on the film so that the electrode spacing is 3-5 mm.
[0010] Preferably, the solvent is one of acetone, methanol, ethanol and acetonitrile, the concentration of the suspension is 1-25 mg / mL; the volume of the suspension measured by the pipette is 2-100 μL.
[0011] On the other hand, the present invention provides a NO2 sensing test method, in which the sensor is fixed in a closed cavity of known volume and connected to an external multimeter and a DC heating power supply. The power of the heating power supply is adjusted to make the sensor work at 50-300°C, and air is used as the background gas to enter the closed cavity at a certain flow rate until the resistance of the sensor is stable. After the resistance is stable, the total flow rate is kept unchanged, and the NO2 gas valve is opened to allow NO2 to fully mix with the air and then enter the closed cavity to contact the sensor. At the same time, the timing is started and the resistance change value of the sensor within the specified time is recorded; after the reaction is completed, the NO2 gas valve is closed to allow the sensor to contact the air, and the resistance begins to recover. A certain recovery time is fixed before the next sensing test is performed; the NO2 gas concentration is changed within the range of 0-200ppm, and the above process is repeated more than 2 times;
[0012] The collected resistance data can be exported through the multimeter program to obtain the change value of the resistance signal over time, with concentration as the horizontal axis and the resistance change rate ΔR (the stable resistance value in air is R a , the final resistance after NO2 contact within the specified time is R g , ΔR=(R g -R a ) / R a ) to obtain the standard curve.
[0013] The volume of the closed cavity is 0.5-2L.
[0014] The response time of the sensor is 1-10 minutes, and the recovery time is 5-60 minutes.
[0015] The total flow rate of the gas through the closed cavity is 100-500 mL / min.
[0016] The present invention has the following advantages:
[0017] (1) The prepared ZnO-NiCo2O4 composite metal oxide as a sensing material has a large specific surface area and porous structure, constructs a pn heterojunction, and lays a structural foundation for good sensing performance.
[0018] (2) Compared with the traditional semiconductor gas sensor, the NO2 sensor of the present invention can fix the sensing film on the ceramic tube by a simple method (drip coating). The method is simple and has good processability, which solves the problem that the traditional gas sensor requires high-temperature sintering and complex processing.
[0019] (3) Compared with other existing semiconductor metal oxide sensors, the sensor of the present invention can eliminate the interference of volatile organic compounds, and has high selectivity (for the same concentration of 20 ppm of the test gas, the response value ΔR of NO2 is as high as 55%, while the response values of other common volatile organic compounds such as methanol and ethanol are all lower than 30%) and high sensitivity (it has a sensitive response to 5 ppm NO2, with a response value R as high as 32%, and the response increases with the increase of NO2 concentration). It has the advantages of good response recovery and repeatability, and can meet the detection needs of trace NO2 gas in the presence of multiple interfering gases.
[0020] (4) The sensor of the present invention has a wide operating temperature range and is portable. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the response sensitivity change curve of the sensor prepared in Example 1 to 20 ppm NO2 at 80-160°C.
[0022] Figure 2 This is the response sensitivity change curve of the sensor prepared in Example 2 to 0-20 ppm NO2 at 100°C.
[0023] Figure 3 This is the selectivity graph of the sensor prepared in Example 3 to 20 ppm of different gases at 100°C.
[0024] Figure 4This is the repeatability graph of the sensor prepared in Example 4 for 20 ppm NO2 at 100°C.
[0025] Figure 5 This is the adsorption-desorption curve of material ZnO-NiCo2O4. DETAILED DESCRIPTION
[0026] The present invention will be described in detail below in conjunction with the accompanying drawings and embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.
[0027] A method for detecting NO2 using a composite metal oxide ZnO-NiCo2O4 as a sensor includes sensor preparation, NO2 sensing test, data collection and collation, and the specific steps are as follows:
[0028] (1) Preparation of the sensor: The composite metal oxide ZnO-NiCo2O4 is dispersed in a solvent to make it uniformly dispersed, and the uniformly dispersed suspension is transferred using a pipette to prepare a film, and parallel electrodes are arranged on the film with an electrode spacing of 3-5 mm;
[0029] (2) NO2 sensing test: Fix the prepared sensor in a closed cavity of known volume, and connect it to an external multimeter and a DC heating power supply. Adjust the power of the heating power supply to make the sensor work at 50-300°C. Use air as the background gas and allow it to enter the closed cavity at a certain flow rate until the resistance of the sensor stabilizes. After the resistance stabilizes, keep the total flow rate unchanged, open the NO2 gas valve, and allow NO2 to fully mix with the air and then enter the closed cavity to contact the sensor. Start timing at the same time and record the resistance change value of the sensor within the specified time; after the reaction is completed, close the NO2 gas valve to allow the sensor to contact the air, and the resistance begins to recover. Fix a certain recovery time before conducting the next sensing test; change the NO2 gas concentration within the range of 0-200ppm, and repeat the above process more than 2 times;
[0030] (3) Data collection and organization: The collected resistance data can be exported through the multimeter program to obtain the change value of the resistance signal over time, with concentration as the horizontal axis and the resistance change rate ΔR (the stable resistance value in air is R a The final resistance after NO2 contact within the specified time is Rg, ΔR=(R g -R a ) / R a ), and obtain the standard curve;
[0031] In the step (1), the dispersion solvent is one of acetone, methanol, ethanol and acetonitrile, and the concentration of the suspension is 1-25 mg / mL; the volume of the suspension measured by the pipette is 2-100 μL;
[0032] The volume of the sealed cavity in step (2) is 0.5-2L;
[0033] The response time of the sensor in step (2) is 1-10 min, and the recovery time is 5-60 min;
[0034] In step (2), the total flow rate of the gas through the closed cavity is 100-500 mL / min;
[0035] ZnO-NiCo2O4 is prepared by a three-step hydrothermal hydrolysis and calcination method. The nickel source, cobalt source and glycerol undergo hydrothermal reaction to obtain bimetallic glycerol nanospheres. The nanospheres are hydrolyzed in a certain concentration of zinc nitrate solution for surface modification and finally calcined to obtain composite metal oxides, which are uniform microspheres with a rough surface, macropores and mesopores with a size of 400-500nm.
[0036] The preparation method of ZnO-NiCo2O4 composite metal oxide is as follows: weigh 0.1mmol nickel nitrate solid and 0.1mmol cobalt nitrate solid and dissolve them in 40mL isopropanol, add 8mL glycerol during stirring, stir and ultrasonically oscillate to fully mix, transfer the solution to a reactor, and hydrothermally react at 180°C for 10h. The reaction product is washed with isopropanol and vacuum dried, and then placed in 20mL 0.01mol / L zinc nitrate solution and stirred for 6h for hydrolysis. After hydrolysis, the product is washed and dried with isopropanol, heated to 400°C at 2°C / min in a tube furnace, and annealed for 3h to obtain ZnO-NiCo2O4 composite metal oxide.
[0037] The sensing principle of NO2 by composite metal oxides is: in the air, O2 captures electrons in the conduction band of the material for surface adsorption; in the NO2 atmosphere, NO2 with strong electrophilicity competes with O2 to capture electrons, causing resistance changes; returning to the air, NO2 desorbs and the resistance returns. ZnO is a typical n-type semiconductor, NiCo2O4 is a p-type semiconductor, holes flow to NiCo2O4, electrons flow to ZnO, forming a pn junction at the contact interface, reducing the height of the potential barrier, thereby reducing the resistance of the sensor and improving the sensing response. The response value ΔR is used as a measure of the sensitivity of the material to the gas to be measured, and the stable resistance value in the air is R a The final resistance after contacting with the gas to be measured within the specified time is R g , ΔR=(R g -R a ) / R a The larger the ΔR value is, the better the material responds to the gas to be tested.
[0038] The change in resistance is proportional to the concentration of NO2 within a certain range. This multi-metal oxide has a large specific surface area, which is conducive to gas adsorption and the increase of reaction sites; the coexistence of macropores and mesopores is conducive to gas transmission and diffusion; ZnO and NiCo2O4 form a pn heterojunction, which enhances conductivity and is conducive to gas adsorption and sensing.
[0039] Example 1
[0040] Sensor test on NO2 working temperature: Weigh 5mg ZnO-NiCo2O4 composite metal oxide sample into a 5mL centrifuge tube, add 1.5mL anhydrous ethanol, and ultrasonicate for 20min. Take 30μL of suspension with a pipette, evenly apply it on the ceramic tube, and dry it in an oven at 40℃ for 30min. Fix the prepared sensor in a 500mL blue-capped bottle and connect it to an external multimeter and DC power supply. Adjust the power of the DC power supply to make the ceramic tube work at a certain temperature. Pass air at a flow rate of 400mL / min into the blue-capped bottle. After the resistance remains stable, reduce the air flow rate to 300mL / min, open the NO2 gas valve and adjust the flow rate to 100mL / min. The total flow rate remains unchanged, and the timing is 10min as the response time. After the reaction is completed, close the NO2 gas valve, restore the air flow rate to 400mL / min, make the sensor contact with fresh air, and the resistance decreases. The timing is until the resistance returns to the initial state. After the response is completed, the collected resistance data is exported through the multimeter program to obtain the change value of the resistance signal over time. The temperature is used as the horizontal axis and the change rate of the resistance signal ΔR is used as the vertical axis to obtain the working curve, as shown in the figure. Figure 1 shown.
[0041] Example 2
[0042] Sensor test on NO2 concentration: Weigh 5mg ZnO-NiCo2O4 composite metal oxide sample into a 5mL centrifuge tube, add 1.5mL anhydrous ethanol, and ultrasonicate for 20min. Use a pipette to take 30μL of the suspension, evenly apply it on the ceramic tube, and dry it in an oven at 40℃ for 30min. Fix the prepared sensor in a 500mL blue-capped bottle and connect it to an external multimeter and DC power supply. Adjust the power of the DC power supply so that the ceramic tube works at 100℃. Pass air at a flow rate of 400mL / min into the blue-capped bottle. After the resistance remains stable, reduce the air flow rate, open the NO2 gas valve to adjust the flow rate, and keep the total flow rate unchanged. At the same time, count 10min as the response time. After the reaction is completed, close the NO2 gas valve, restore the air flow rate to 400mL / min, so that the sensor is in contact with fresh air and the resistance decreases. Due to the long recovery time, set the recovery time to 15min. . After the response is completed, the collected resistance data is exported through the multimeter program to obtain the change value of the resistance signal over time. The working curve is obtained by plotting the time as the horizontal axis and the change rate of the resistance signal ΔR as the vertical axis. Figure 2 shown.
[0043] Example 3
[0044] Sensor selectivity test for NO2: Weigh 5 mg ZnO-NiCo2O4 composite metal oxide sample into a 5 mL centrifuge tube, add 1.5 mL anhydrous ethanol, and ultrasonicate for 20 minutes. Use a pipette to take 30 μL of the suspension, evenly apply it on the ceramic tube, and dry it in an oven at 40°C for 30 minutes. Fix the prepared sensor in a 500 mL blue-capped bottle and connect it to an external multimeter and DC power supply. Adjust the power of the DC power supply so that the ceramic tube works at 100°C. Pass air at a flow rate of 400 mL / min into the blue-capped bottle. After the resistance remains stable, reduce the air flow rate to 300 mL / min, open the H2S gas valve and adjust the flow rate to 100 mL / min. The total flow rate remains unchanged, and the timing is 10 minutes as the response time. After the reaction is completed, close the H2S gas valve, restore the air flow rate to 400 mL / min, allow the sensor to contact with fresh air, and the resistance drops. Timing is until the resistance returns to the initial state. The same sensing test is carried out for CO, CO2, NO, methanol, ethanol, acetone, and trimethylamine. After the response is completed, the collected resistance data is exported through the multimeter program to obtain the change value of the resistance signal over time. The gas type is used as the horizontal axis and the change rate of the resistance signal ΔR is used as the vertical axis to obtain the working curve, such as Figure 3 shown.
[0045] Example 4
[0046] Sensor test on NO2 working temperature: Weigh 5mg ZnO-NiCo2O4 composite metal oxide sample into a 5mL centrifuge tube, add 1.5mL anhydrous ethanol, and ultrasonicate for 20min. Use a pipette to take 30μL of the suspension, evenly apply it on the ceramic tube, and dry it in an oven at 40℃ for 30min. Fix the prepared sensor in a 500mL blue-capped bottle and connect it to an external multimeter and DC power supply. Adjust the power of the DC power supply so that the ceramic tube works at 100℃. Pass air at a flow rate of 400mL / min into the blue-capped bottle. After the resistance remains stable, reduce the air flow rate to 300mL / min, open the NO2 gas valve and adjust the flow rate to 100mL / min. The total flow rate remains unchanged, and the timing is 10min as the response time. After the reaction is completed, close the NO2 gas valve, restore the air flow rate to 400mL / min, so that the sensor is in contact with fresh air, the resistance decreases, and the timing is until the resistance returns to the initial state. This cycle is repeated 7 times. After the response is completed, the collected resistance data is exported through the multimeter program to obtain the change value of the resistance signal over time. The number of cycles is used as the horizontal axis and the change rate of the resistance signal ΔR is used as the vertical axis to obtain the working curve, as shown in the figure. Figure 4 shown.
Claims
1. A method for detecting NO2 using a semiconductor sensor, characterized in that: The composite metal oxide ZnO-NiCo2O4 is used as the sensing membrane of the semiconductor sensor; The composite metal oxide ZnO-NiCo2O4 has macropores and mesopores, and the microscopic morphology is microspheres with an average particle size of 400-500nm.
2. The method according to claim 1, characterized in that The preparation method of the composite metal oxide ZnO-NiCo2O4 is to subject raw materials containing a nickel source and a cobalt source to a hydrothermal reaction, hydrolyze them in a zinc salt solution, and finally calcine them to obtain the composite metal oxide.
3. The method according to claim 2, characterized in that The preparation method of the composite metal oxide ZnO-NiCo2O4 comprises the following steps: subjecting a nickel source, a cobalt source and glycerol to a hydrothermal reaction to obtain bimetallic glycerol nanospheres, subjecting the nanospheres to a hydrolysis reaction in a zinc nitrate solution, and finally calcining to obtain the composite metal oxide.
4. The method according to claim 1, characterized in that: The method for preparing the semiconductor sensor comprises the following steps: The composite metal oxide ZnO-NiCo2O4 is dispersed in a solvent to make it uniformly dispersed, and a pipette is used to transfer the uniformly dispersed suspension to prepare a film, and parallel electrodes are arranged on the film with an electrode spacing of 3-5 mm.
5. The method according to claim 4, characterized in that The solvent is one of acetone, methanol, ethanol and acetonitrile; the concentration of the suspension is 1-25 mg / mL; the volume of the suspension measured by the pipette is 2-100 μL.
6. The method according to claim 1, characterized in that The NO2 sensor test method is as follows: fix the sensor in a closed cavity of known volume, connect it to an external multimeter and a DC heating power supply, adjust the heating power supply power, and make the sensor o C, with air as the background gas, entering the closed cavity at a certain flow rate until the resistance of the sensor is stable. After the resistance is stable, keep the total flow rate unchanged, open the NO2 gas valve, allow NO2 to fully mix with air and enter the closed cavity to contact the sensor, start timing at the same time, and record the resistance change value of the sensor within the specified time; after the reaction is completed, close the NO2 gas valve, allow the sensor to contact with air, and the resistance begins to recover. After a certain recovery time, perform the next sensor test; change the NO2 gas concentration within the range of 0-200 ppm, and repeat the above process more than 2 times; The collected resistance data can be exported through the multimeter program to obtain the change value of the resistance signal over time, with concentration as the horizontal axis and the resistance change rate ΔR. The stable resistance value in the air is R a , the final resistance after NO2 contact within the specified time is R g , ΔR=(R g -R a ) / R a , and obtain the standard curve.
7. The method according to claim 6, characterized in that The volume of the closed cavity is 0.5-2L.
8. The method according to claim 6, characterized in that The response time of the sensor is 1-10 minutes, and the recovery time is 5-60 minutes.
9. The method according to claim 6, characterized in that The total flow rate of gas through the closed cavity is 100-500mL / min.