Preparation of a thioquinoline-amine metal compound and its application in high-temperature solution polymerization of olefins

By designing thioquinoline-amino titanium, zirconium and hafnium metal compounds, the problem of the reduction of existing catalysts at high temperatures is solved, and the catalytic performance of high activity and high temperature resistance is achieved. It is suitable for polymerization of olefins at high temperature solutions, and has improved the Preparation capacity of polyolefin materials.

CN114671901BActive Publication Date: 2024-11-22QINGDAO UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210274038.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-20
Publication Date
2024-11-22
Estimated Expiration
2042-03-20

AI Technical Summary

Technical Problem

The existing metal-based catalysts have problems of reduced activity and insufficient durability when used at high temperatures, and it is difficult to meet the needs of industrial polyethylene catalysts. Especially in the high-temperature solution polymerization process, there is a lack of stable and easy-to-prepared new catalysts.

Method used

New thioquinoline-amino titanium, zirconium and hafnium metal compounds were designed and prepared. By changing the substituents of the structure, they regulate the steric hindrance and electronic effects of the catalyst, and developed a high-activity and high-temperature resistance catalyst suitable for olefin high-temperature solutions. polymerization.

Benefits of technology

It achieves catalytic properties with high activity (up to 108g(PE)·mol-1(cat)·h-1) and high temperature resistance (210℃). It is suitable for the preparation of polyolefin elastomers, and enhances the high level of polyolefins in the international high-end Competitiveness in the molecular material technology market.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003555130280000021
    Figure BDA0003555130280000021
  • Figure FHA0000007195620000011
    Figure FHA0000007195620000011
  • Figure HDA0003555130290000011
    Figure HDA0003555130290000011
Patent Text Reader

Abstract

The present invention relates to the preparation of a thioquinoline-amine metal compound and its application in high-temperature solution polymerization of olefins. The present invention introduces a thioquinoline skeleton, designs and synthesizes novel thioquinoline-amine titanium, zirconium, and hafnium metal compounds, and by changing substituents of different structures, the steric effect and electronic effect of the model metal catalyst can be conveniently regulated to achieve different catalytic properties. The novel thioquinoline zirconium and hafnium metal compounds reported in the present invention have mature preparation methods, high activity (up to 10 8 g(PE)·mol ‑1 (cat) h ‑1 ), high temperature resistance (210°C), and good copolymerization performance, and are suitable for preparing polyolefin elastomers through high temperature solution polymerization of olefins. Therefore, the thioquinoline-amino titanium, zirconium, and hafnium metal compounds reported in the present invention have excellent high temperature resistance, original innovation, and can enhance my country's competitiveness in the international high-end polyolefin polymer material technology market.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the preparation of a thioquinoline-amine metal compound and the application of the olefin high-temperature solution polymerization thereof. Background Art

[0002] Over the past few decades, polyolefins have become the largest volume synthetic polymers. For example, more than 70 million tons of polyethylene are produced annually, of which about 1 million tons. 77% are produced using metal-based catalysts. Therefore, the development of new metal-based catalysts has attracted great interest from academia and industry to prepare new polyolefin products and improve current polymerization processes. Usually, these catalysts should contain ligand-stabilized ligand structures that are inexpensive, easy to prepare and systematic. In addition, high activity and high temperature resistance are usually key features when industrializing. So far, there are still relatively few stable ligand structures that can meet all the above requirements. At present, industrial polyethylene catalysts include Ziegler-Natta catalysts (DE Pat 889229 (1953); IT Pat 545332 (1956) and IT Pat 536899 (1955)), Phillips catalysts (Belg. Pat. 530617 (1955)) and metallocene catalysts (W. Kaminsky, Metalorganic Catalysts for Synthesis and Polymerization, Berlin: Springer, 1999), and non-metallocene catalysts that have attracted more and more attention in recent years (Arriola, DJ, Catalytic Production of Olefin Block Copolymers via Chain Shuttling Polymerization, 2006). High temperature resistant catalysts are the key to preparing polyolefin elastomer POE by high temperature solution polymerization. In 2011, the Jerzy research group and in 2012, the Philip P research group reported that aminoquinoline zirconium and hafnium complexes catalyzed olefin polymerization (Organometallics 2011, 30, 251–262; Organometallics 2012, 31, 6244-6251), respectively. The copolymerization of ethylene and 1-octene has high activity and high temperature resistance, and is suitable for high temperature solution polymerization process.

[0003] The present invention relates to the preparation of a thioquinoline-amine metal compound and its application in high-temperature solution polymerization of olefins. The present invention introduces a thioquinoline skeleton, designs and synthesizes a novel thioquinoline-amine titanium, zirconium, and hafnium metal compound. By changing the substituents of different structures, the steric effect and electronic effect of the model metal catalyst can be conveniently regulated to achieve different catalytic properties. The novel thioquinoline-amine zirconium and hafnium metal compounds reported in the present invention have mature preparation methods, high activity (up to 10 8 g(PE)·mol -1 (cat) h -1 ), high temperature resistance (210°C), and good copolymerization performance, and are suitable for preparing polyolefin elastomers through high temperature solution polymerization of olefins. Therefore, the thioquinoline-amino titanium, zirconium, and hafnium metal compounds reported in the present invention have excellent high temperature resistance, original innovation, and can enhance my country's competitiveness in the international high-end polyolefin polymer material technology market. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing thioquinoline-amino zirconium and hafnium metal compounds and their application in olefin polymerization.

[0005] The present invention provides a thioamide quinoline titanium, zirconium, or hafnium metal compound represented by formula (I):

[0006]

[0007] Wherein, M is selected from titanium, zirconium, and hafnium; R 1 is selected from methyl, ethyl, hydrogen, isopropyl, chloro; R 2 is selected from methyl, methoxy, hydrogen; R 3 is selected from ethyl, tert-butyl, isopropyl, 2,6-dimethylphenyl; R 4 is selected from hydrogen, methyl, tert-butyl, isopropyl, 2,6-diisopropylphenyl, 2-isopropylphenyl; X is selected from methyl, chlorine, dimethylamino.

[0008] Preferably, the metal compound of the present invention is selected from any one of the following complexes:

[0009] Hf1:M=Hf,R 1 = isopropyl, R 2 =Hydrogen, R 3 = isopropyl, R 4 = methyl, X = methyl;

[0010] Zr1: M = Zirconium, R 1 = isopropyl, R 2 =Hydrogen, R 3 = isopropyl, R 4 = methyl, X = methyl;

[0011] Hf2:M=Hafnium, R 1 = isopropyl, R 2 =Hydrogen, R 3 =2,6-dimethylphenyl, R 4 = methyl, X = methyl;

[0012] Zr2: M = Zirconium, R 1 = isopropyl, R 2 =Hydrogen, R 3 =2,6-dimethylphenyl, R 4 = methyl, X = methyl.

[0013] The present invention provides a method for preparing the above-mentioned thioquinoline-amino titanium, zirconium, and hafnium metal compounds, comprising the following steps:

[0014] The metal chloride is dissolved in 30-100 mL of anhydrous solvent, 4.0-5.0 molar equivalents of methylmagnesium bromide are added, and the mixture is stirred at -40°C for 2 hours under nitrogen protection, and then 1 molar equivalent of thioquinoline-amine ligand is added, and stirring is continued for 5 hours; the solvent is removed under reduced pressure, and extraction is performed with a good solvent to obtain a thioquinoline-amine metal compound.

[0015] In the above preparation method, the anhydrous solvent is selected from benzene, toluene, xylene, and n-hexane; and the good solvent is selected from n-hexane, n-pentane, n-heptane, cyclohexane, and toluene.

[0016] The present invention also provides the use of the thioquinoline-amino titanium, zirconium and hafnium metal compounds shown in the above formula (I) in catalyzing olefin polymerization reactions.

[0017] In the above application, the olefin is one or more of ethylene, propylene, styrene, 1-butene, 1-hexene and 1-octene.

[0018] The catalyst is further added with a co-catalyst, which is one or more of tripentafluorophenyl boron, triphenylcarbonium tetrakis(pentafluorophenyl)borate, aluminoxane, alkyl aluminum and alkyl aluminum chloride. The aluminoxane is methyl aluminumoxane, ethyl aluminumoxane or isobutyl aluminumoxane; the alkyl aluminum is trimethyl aluminum, triethyl aluminum, triisobutyl aluminum or tri-n-hexyl aluminum; the alkyl aluminum chloride is diethyl aluminum monochloride, diethyl aluminum sesquichloride or ethyl aluminum dichloride.

[0019] In the above polymerization reaction, the polymerization temperature is 0-210° C., the polymerization pressure is 0.1-5 MPa, and the polymerization solvent is one or more of toluene, hexane, and heptane.

[0020] The present invention provides the preparation of thioquinoline-amido titanium, zirconium, hafnium metal compounds and the application of the compounds in catalyzing olefin polymerization. The novel thioquinoline-amido titanium, zirconium, hafnium metal compounds reported in the present invention have the advantages of simple preparation, high activity (up to 10 8 g(PE)·mol -1 (cat) h -1 ), high temperature resistance (210℃), and good copolymerization performance, it is suitable for the preparation of polyolefin elastomers by high temperature solution polymerization of olefins. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 is the crystal structure diagram of the complex Hf1; Figure 2 This is the crystal structure diagram of the complex Zr1. DETAILED DESCRIPTION

[0022] The present invention is further described by way of examples, but the present invention is not limited thereto. The examples of the present invention can enable those skilled in the art to understand the present invention more comprehensively.

[0023] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0024] The thioquinoline-amine ligand in the present invention is synthesized according to the method reported in the document Macromolecules 2022, DOI: 10.1021 / acs.macromol.1c02351.

[0025] The present invention is described below with reference to specific embodiments.

[0026] Example 1. Preparation of Compound Hf1

[0027] Weigh hafnium tetrachloride (0.352g, 1.1mmol), add 10mL dry toluene, slowly add 1.6mL / 4.8mmol methylmagnesium bromide solution (3M) at -40℃ (acetonitrile liquid nitrogen bath), and stir for 2 hours. Add 8-[N-(2,6-diisopropyl-aniline)=CH]-2-(isopropylthio)-quinoline (0.39g / 1mmol), stir for two hours at -40℃, return to room temperature, and stir for 5 hours. Protect from light. Remove the solvent, extract with toluene, filter, and obtain 0.5g of product with a yield of 79%. 1H NMR (400MHz, C6D6): δ7.47(dd,J=7.3and 1.4Hz,1H),7.39-7.36(m,1H),7.30-7.26(m,3H),7.07(dd,J=8.1and 1.3Hz,1H),6.85(t,J=7.7Hz,1H),6.59(d,J=8.4Hz,1H),4.93(q,J=6.8Hz,1H,CH(CH3)-N),4.62(sept,J=6.6Hz,1H,S-CH(CH3)2),3.57(s ept,J=6.8Hz,1H,Ar-CH(CH3)2),3.40(sept,J=6.8Hz,1H,Ar-CH(CH3)2),1.84(d,J=6.7Hz,3H),1.51(d,J=6.8Hz,3H),1.43(dd,J=5.8and 4.1Hz,6H,Hf-Me),1.32(d,J=6.9Hz,3H),0.95(d,J=6.8Hz,3H),0.78(s,3H,Hf-Me),0.45(d,J=6.7Hz,6H),0.14(s,3H,Hf-Me)ppm. 13 C NMR (400MHz, C6D6): δ173.55,150.17,149.50,146.34,146.21,139.23,138.22,130.34,129.74,127.94,126.05 125.51,125.29,124.45,119.34,74.53(NCHCH3),60.18(Hf-Me),48.35(Hf-Me),4 4.67(Hf-Me),41.59,28.44,27.82,26.64,26.27,26.17,25.56,22.77,20.99ppm.

[0028] Example 2. Preparation of Compound Zr1

[0029] Weigh zirconium tetrachloride (0.256g, 1.1mmol), add 10mL dry toluene, slowly add 1.6mL / 4.8mmol methylmagnesium bromide solution (3M) at -40℃ (acetonitrile liquid nitrogen bath), and stir for 2 hours. Add 8-[N-(2,6-diisopropyl-aniline)=CH]-2-(isopropylthio)-quinoline (0.39g / 1mmol), stir for two hours at -40℃, return to room temperature, and stir for 5 hours. Protect from light. Remove the solvent, extract with toluene, filter, and obtain 0.48g of product with a yield of 88%. 1H NMR (400MHz, C6D6): δ7.48 (dd, J=7.2and 1.2Hz,1H),7.40-7.36(m,1H),7.30-7.28(m,3H),7.01(d,J=8.0Hz,1H),6.88(t,J=7.7Hz,1H),6.62(d,J=8.5Hz,1H) ,4.99(q,J=6.8Hz,1H,CH(CH3)-N),4.52(sept,J=6.7Hz,1H,S-CH(CH3)2),3.59(sept,J=6.8Hz,1H,Ar-CH(CH3)2),3. 33(sept,J=7.8Hz,1H,Ar-CH(CH3)2),1.79(d,J=6.7Hz,3H),1.43-1.46(m,6H),1.38(d,J=6.8Hz,3H),1.33(d,J=6.8 Hz,3H),0.95(s,3H,Zr-Me),0.91(d,J=6.8Hz,3H),0.76(s,3H,Zr-Me),0.49(d,J=6.8Hz,3H),0.38(s,3H,Zr-Me)ppm. 13 C NMR (400MHz, C6D6): δ172.85,149.17,146.31,146.23,138.96,137.95,130.32,129.67,128.18,127.94,126.00,125.45,1 25.30,124.37,119.57,73.19(NCHCH3),42.49(Zr-Me),28.74,28.01,26.72,26.42,26.23,25.71,25.38,22.61,21.43ppm.

[0030] Example 3. Preparation of Compound Hf2

[0031] Weigh hafnium tetrachloride (0.352g, 1.1mmol), add 10mL dry toluene, slowly add 1.6mL / 4.8mmol methylmagnesium bromide solution (3M) at -40℃ (acetonitrile liquid nitrogen bath), and stir for 2 hours. Add 8-[N-(2,6-diisopropyl-aniline)=CH]-2-(2,6-dimethylphenylthio)-quinoline (0.452g / 1mmol), stir for two hours at -40℃, return to room temperature, and stir for 5 hours. Protect from light. Remove the solvent, extract with toluene, filter, and obtain 0.52g of product with a yield of 75%. 1H NMR (400MHz, C6D6): δ7.36-7.29(m,3H),7.27-7.25(m,2H),7.00(dd,J=8.1and 1.2Hz,1H),6.90-6.84(m,2H),6.70(t,J=7.7Hz,1H),6.64-6.60(m,2H),5.15(q,J=6.8Hz,1H,CH(CH3)-N),4.54(sept,J=6.7Hz,1H,Ar-CH(CH3)2 ),3.75(sept,J=6.7Hz,1H,Ar-CH(CH3)2),2.64(s,3H),1.70(d,J=6.7Hz,3H),1.52(d,J=6.70Hz,3H),1.44-1.36(m,12H),0.45(s,9H,Hf-Me)ppm. 13 C NMR (400MHz, C6D6): δ172.94,149.31,147.94,146.54 146.27,139.26,135.91,134.83,134.34,129.49,126.99,125.61,125.34,124.46,119. 73,73.95(NCHCH3),28.59,27.84,26.75,26.46,26.16,26.09,25.52,22.84,21.87ppm.

[0032] Example 4. Preparation of Compound Zr2

[0033] Weigh zirconium tetrachloride (0.256g, 1.1mmol), add 10mL dry toluene, slowly add 1.6mL / 4.8mmol methylmagnesium bromide solution (3M) at -40℃ (acetonitrile liquid nitrogen bath), and stir for 2 hours. Add 8-[N-(2,6-diisopropyl-aniline)=CH]-2-(2,6-dimethylphenylthio)-quinoline (0.452g / 1mmol), stir for two hours at -40℃, return to room temperature, and stir for 5 hours. Protect from light. Remove the solvent, extract with toluene, filter, and obtain 0.52g of product with a yield of 75%. 1H NMR (400MHz, C6D6): δ7.33-7.22(m,5H),7.06(dd,J=8.1and 1.2Hz,1H),6.91-6.85(m,2H),6.73(t,J=7.7Hz,1H),6.68-6.61(m,2H),5.25(q,J=6.9Hz,1H,CH(CH3)-N),4.41(sept,J=6.7Hz,1H,Ar-CH( CH3)2),3.77(sept,J=6.2Hz,1H,Ar-CH(CH3)2),2.58(s,3H),1.61(d,J=6.7Hz,3H),1.56(s,3H),1.50(d,J=6.7Hz,3H),1.36(dd,J=6.8and 3.0Hz,9H),0.69(s,9H,Zr-Me)ppm. 13 C NMR (400MHz, C6D6): δ170.78,146.60,145.85,145.54,145.31,137.70,133.56,132.99,128.13,127.86,124.41,124.0 3,123.19,118.80,70.80(NCHCH3),40.39(Zr-Me),27.73,26.89,25.56,24.94,24.87,24.16,24.11,21.61,20.79ppm.

[0034] Example 5: Hf1-catalyzed ethylene / 1-octene copolymerization (130°C)

[0035] A 5L steel reactor was used in the polymerization. Before use, the polymerization kettle was evacuated and replaced with nitrogen 3 to 5 times at 120°C. Under vacuum, when the temperature dropped below 90°C, the n-hexane valve was opened in the 5L reactor to add about 700g of n-hexane solvent by ethylene pressure, then the n-hexane valve was closed, the 1-octene valve was opened, and 200g of 1-octene comonomer was introduced, then the 1-octene valve was closed, and the agitator was turned on, the speed was set, and the mixture of n-hexane and 1-octene was fully stirred. The reaction temperature was set and waited for the temperature to rise. The mixture in the reactor was heated to 130°C. When this temperature was reached, the reactor was saturated with 2.7MPa of ethylene, and 10μmol of catalyst, co-catalyst and the required amount of MAO were quickly transferred directly to the catalyst addition tank by syringe and single needle through stainless steel tube, and the n-hexane valve was opened to make its pressure just greater than the pressure in the kettle, so as to press the catalyst and co-catalyst into the polymerization reactor. The polymerization conditions were maintained for 10 minutes, and the valve on the ethylene cylinder was adjusted to 2.7 MPa and ethylene was always passed to maintain the pressure in the reactor. The heat was continuously discharged from the reaction vessel through the deionized water circulated by the water pump into the internal cooling coil. After the reaction was completed, the ethylene was turned off, and the resulting reaction solution was released from the bottom of the reactor into a large beaker, quenched with isopropanol or ethanol, and hydrochloric acid was added to remove the salt generated by the quenching metal aluminum. After filtering the polymer, it was washed with ethanol, vacuum dried to constant weight, and weighed. Polymerization activity: 2.21×10 8 g·mol -1 (Hf) h -1 , polymer Mw = 567 kg·mol -1 , Mw / Mn=1.8, the 1-octene content in the copolymer is 8.5 mol%.

[0036] Example 6: Zr1-catalyzed ethylene / 1-octene copolymerization (130°C)

[0037] The polymerization process and reaction conditions were the same as in Example 5, and the catalyst used was Zr1. Polymerization activity: 2.55×10 7 g·mol -1 (Zr)·h -1 , polymer Mw = 361 kg·mol -1 , Mw / Mn=2.6, the 1-octene content in the copolymer is 8.0 mol%.

[0038] Example 7: Hf2-catalyzed ethylene / 1-octene copolymerization (130°C)

[0039] The polymerization process and reaction conditions were the same as in Example 5, and the catalyst used was Hf2. Polymerization activity: 3.18×10 8 g·mol -1 (Hf) h -1 , polymer Mw = 300 kg·mol-1 , Mw / Mn=2.4, the 1-octene content in the copolymer is 9.3 mol%.

[0040] Example 8: Zr2-catalyzed ethylene / 1-octene copolymerization (130°C)

[0041] The polymerization process and reaction conditions were the same as in Example 5, and the catalyst used was Zr2. Polymerization activity: 1.07×10 8 g·mol -1 (Zr)·h -1 , polymer Mw = 211 kg·mol -1 , Mw / Mn=2.1, the 1-octene content in the copolymer is 7.3 mol%.

[0042] Example 9: Hf1-catalyzed ethylene / 1-octene copolymerization (150°C)

[0043] A 5L steel reactor was used in the polymerization. Before use, the polymerization kettle was evacuated and replaced with nitrogen at 120°C for 3 to 5 times. Under vacuum, when the temperature dropped below 90°C, the n-hexane valve was opened in the 5L reactor to add about 700g of n-hexane solvent by ethylene pressure, then the n-hexane valve was closed, the 1-octene valve was opened, and 200g of 1-octene comonomer was introduced, then the 1-octene valve was closed, and the agitator was turned on, the speed was set, and the mixture of n-hexane and 1-octene was fully stirred. The reaction temperature was set and waited for the temperature to rise. The mixture in the reactor was heated to 150°C. When this temperature was reached, the reactor was saturated with 2.7MPa of ethylene, and 10μmol of catalyst, co-catalyst and the required amount of MAO were quickly transferred directly to the catalyst addition tank by syringe and single needle through stainless steel tube, and the n-hexane valve was opened to make its pressure just greater than the pressure in the kettle, so as to press the catalyst and co-catalyst into the polymerization reactor. The polymerization conditions were maintained for 10 minutes, and the valve on the ethylene cylinder was adjusted to 2.7 MPa and ethylene was always passed to maintain the pressure in the reactor. The heat was continuously discharged from the reaction vessel through the deionized water circulated by the water pump into the internal cooling coil. After the reaction was completed, the ethylene was turned off, and the resulting reaction solution was released from the bottom of the reactor into a large beaker, quenched with isopropanol or ethanol, and hydrochloric acid was added to remove the salt generated by the quenching metal aluminum. After filtering the polymer, it was washed with ethanol, vacuum dried to constant weight, and weighed. Polymerization activity: 2.57×10 8 g·mol -1 (Hf) h -1 , polymer Mw = 575 kg·mol -1 , Mw / Mn=2.7, the 1-octene content in the copolymer is 8.0 mol%.

[0044] Example 10: Zr1-catalyzed ethylene / 1-octene copolymerization (150°C)

[0045] The polymerization process and reaction conditions were the same as in Example 9, and the catalyst used was Zr1. Polymerization activity: 1.46×10 7 g·mol -1 (Zr)·h -1 , polymer Mw = 261 kg·mol -1 , Mw / Mn=2.3, the 1-octene content in the copolymer is 6.5 mol%.

[0046] Example 11: Hf2-catalyzed ethylene / 1-octene copolymerization (150°C)

[0047] The polymerization process and reaction conditions were the same as in Example 9, and the catalyst used was Hf2. Polymerization activity: 9.06×10 7 g·mol -1 (Hf) h -1 , polymer Mw = 314 kg·mol -1 , Mw / Mn=2.6, and the 1-octene content in the copolymer is 6.3 mol%.

[0048] Example 12: Zr2-catalyzed ethylene / 1-octene copolymerization (150°C)

[0049] The polymerization process and reaction conditions were the same as in Example 9, and the catalyst used was Zr2. Polymerization activity: 7.08×10 6 g·mol -1 (Zr)·h -1 , polymer Mw = 171 kg·mol -1 , Mw / Mn=2.6, and the 1-octene content in the copolymer is 3.1 mol%.

[0050] Example 13: Hf1-catalyzed ethylene / 1-octene copolymerization (180°C)

[0051] A 5L steel reactor was used in the polymerization. Before use, the polymerization kettle was evacuated and replaced with nitrogen 3 to 5 times at 120°C. Under vacuum, when the temperature dropped below 90°C, the n-hexane valve was opened in the 5L reactor to add about 700g of n-hexane solvent by ethylene pressure, then the n-hexane valve was closed, the 1-octene valve was opened, and 200g of 1-octene comonomer was introduced, then the 1-octene valve was closed, and the agitator was turned on, the speed was set, and the mixture of n-hexane and 1-octene was fully stirred. The reaction temperature was set and waited for the temperature to rise. The mixture in the reactor was heated to 180°C. When this temperature was reached, the reactor was saturated with 2.7MPa of ethylene, and 10μmol of catalyst, co-catalyst and the required amount of MAO were quickly transferred directly to the catalyst addition tank by syringe and single needle through stainless steel tube, and the n-hexane valve was opened to make its pressure just greater than the pressure in the kettle, so as to press the catalyst and co-catalyst into the polymerization reactor. The polymerization conditions were maintained for 10 minutes, and the valve on the ethylene cylinder was adjusted to 2.7 MPa and ethylene was always passed to maintain the pressure in the reactor. The heat was continuously discharged from the reaction vessel through the deionized water circulated by the water pump into the internal cooling coil. After the reaction was completed, the ethylene was turned off, and the resulting reaction solution was released from the bottom of the reactor into a large beaker, quenched with isopropanol or ethanol, and hydrochloric acid was added to remove the salt generated by the quenching metal aluminum. After filtering the polymer, it was washed with ethanol, vacuum dried to constant weight, and weighed. Polymerization activity: 2.45×10 8 g·mol -1 (Hf) h -1 , polymer Mw = 550 kg·mol -1 , Mw / Mn=2.2, the 1-octene content in the copolymer is 8.9 mol%.

[0052] Example 14: Hf1-catalyzed ethylene / 1-octene copolymerization (210°C)

[0053] A 5L steel reactor was used in the polymerization. Before use, the polymerization kettle was evacuated and replaced with nitrogen 3 to 5 times at 120°C. Under vacuum, when the temperature dropped below 90°C, the n-hexane valve was opened in the 5L reactor to add about 700g of n-hexane solvent by ethylene pressure, then the n-hexane valve was closed, the 1-octene valve was opened, and 200g of 1-octene comonomer was introduced, then the 1-octene valve was closed, and the agitator was turned on, the speed was set, and the mixture of n-hexane and 1-octene was fully stirred. The reaction temperature was set and waited for the temperature to rise. The mixture in the reactor was heated to 210°C. When this temperature was reached, the reactor was saturated with 2.7MPa of ethylene, and 10μmol of catalyst, co-catalyst and the required amount of MAO were quickly transferred directly to the catalyst addition tank by syringe and single needle through stainless steel tube, and the n-hexane valve was opened to make its pressure just greater than the pressure in the kettle, so as to press the catalyst and co-catalyst into the polymerization reactor. The polymerization conditions were maintained for 10 minutes, and the valve on the ethylene cylinder was adjusted to 2.7 MPa and ethylene was always passed to maintain the pressure in the reactor. The heat was continuously discharged from the reaction vessel through the deionized water circulated by the water pump into the internal cooling coil. After the reaction was completed, the ethylene was turned off, and the resulting reaction solution was released from the bottom of the reactor into a large beaker, quenched with isopropanol or ethanol, and hydrochloric acid was added to remove the salt generated by the quenching metal aluminum. After filtering the polymer, it was washed with ethanol, vacuum dried to constant weight, and weighed. Polymerization activity: 2.10×10 8 g·mol -1 (Hf) h -1 , polymer Mw = 480 kg·mol -1 , Mw / Mn=2.2, the 1-octene content in the copolymer is 11 mol%.

Claims

1. A class of thioquinoline-amine metal compounds, whose structure is shown in formula (I): in, M is selected from zirconium and hafnium; R 1 is selected from isopropyl; R 2 is selected from hydrogen; R 3 is selected from isopropyl, 2,6-dimethylphenyl; R 4 is selected from methyl; X is selected from methyl.

2. The method for preparing the thioquinoline-amine metal compound according to claim 1, comprising the steps of: The metal chloride is dissolved in 30-100 mL of anhydrous solvent, 4.0-5.0 molar equivalents of methylmagnesium bromide are added, and the mixture is stirred at -40°C for 2 hours under nitrogen protection, and then 1 molar equivalent of thioquinoline-amine ligand is added, and stirring is continued for 5 hours; the solvent is removed under reduced pressure, and extraction is performed with a good solvent to obtain a thioquinoline-amine metal compound.

3. The preparation method according to claim 2, characterized in that: The anhydrous solvent is selected from benzene, toluene, xylene, and n-hexane; the good solvent is selected from n-hexane, n-pentane, n-heptane, cyclohexane, and toluene.

4. A method for olefin polymerization, characterized in that: The catalyst of the reaction is the thioquinoline-amine metal compound described in claim 1; the olefin is a mixture of ethylene and 1-octene; the catalyst is further added with a co-catalyst, the co-catalyst is triphenylcarbonium tetrakis(pentafluorophenyl)borate and methylaluminoxane; the polymerization temperature is 0-210°C, the polymerization pressure is 0.1-5MPa, and the polymerization solvent is one or more of toluene, hexane, and heptane.