A method for improving the wettability of molten steel on the surface of thin strip continuous casting rollers
By adding Se element and controlling temperature and rotation speed in thin strip continuous casting, the problem of unstable casting roll surface is solved, continuous and stable production of steel strip and thickness uniformity are achieved, and production efficiency and product quality are improved.
Patent Information
- Application Number
- CN202210343152.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-31
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-03-31
AI Technical Summary
In thin strip continuous casting technology, the molten metal forms unstable strips on the surface of the casting roll and the strip thickness is uneven, causing the strip to break and stop pouring, affecting production efficiency and product quality, and increasing costs.
Add Se element to the molten metal, and control its temperature and the rotation speed of the casting roller to reduce the surface tension and fluctuations of the molten steel, improve the wettability, so that the molten metal can cool evenly on the surface of the casting roller, solidify stably, and form a steel strip with uniform thickness. .
It realizes the continuous production of steel strips, improves production efficiency and product quality, reduces costs, and ensures the stability and thickness uniformity of the steel strips.
Smart Images

Figure CN114799099B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of thin strip continuous casting, and in particular relates to a method for improving the wettability of molten steel on the surface of a thin strip continuous casting roller. Background Art
[0002] Thin strip continuous casting technology is a new type of thin strip steel production process. By adopting a twin-roll continuous casting machine, the molten steel casting process is completed in a molten pool. The molten pool is surrounded by a pair of relatively rotating casting rolls and side sealing plates. The molten metal is introduced between the pair of casting rolls, so that the metal cools and solidifies into a strip on the surface of the rotating casting rolls, and the solidified steel strip product is continuously conveyed downward in the roller gap between the casting rolls.
[0003] Compared with the traditional hot rolling process, the thin strip continuous casting technology has the advantages of simple production process, low energy consumption and low product cost. However, this technology also has certain bottlenecks, mainly in whether the molten metal can be continuously and stably formed into strips and whether the thickness of the strips is uniform. If the molten metal cannot be continuously and stably formed into strips, or the thickness of the strips fluctuates, it is easy to cause the strip to break and stop casting, making it impossible to achieve continuous production, which will affect production efficiency and product quality, and lead to higher costs. Summary of the invention
[0004] The present invention provides an advantageous technical solution, which can improve the wettability of the casting roll surface with molten steel, thereby providing continuity and stability of casting.
[0005] Specifically, the present invention reduces the surface tension of molten steel by adding Se element to the molten metal and controlling the temperature of the molten metal, and reduces the fluctuation of the molten metal on the surface of the casting roll by controlling the linear speed of the casting roll rotation, thereby improving the wettability of the molten metal on the surface of the casting roll. The good wettability of the molten metal can make the molten metal adhere well to the surface of the casting roll, cool evenly, and the thickness of the solidified shell is uniform and stable, so that the strip is stable and the thickness of the steel strip is uniform, and it is not easy to cause the accident of breaking the strip and stopping the casting, so that continuous production can be achieved, the production efficiency and product quality can be improved, and the product cost can be reduced.
[0006] The present invention discloses an improved method for producing thin strip steel, comprising the following steps: molten metal flows to a pair of casting rolls of a twin-roll continuous casting machine, and forms a molten pool above the roller gap between the pair of casting rolls and above the casting surface of the casting rolls, wherein the selenium (Se) content in the molten metal in the molten pool is ≥0.005% by weight, and the temperature of the molten metal in the molten pool is ≥1550°C, the pair of casting rolls rotate relatively, the molten metal in the molten pool cools and solidifies on the casting surface of the casting rolls, and passes downward through the roller gap between the pair of casting rolls to form a steel strip, wherein the rotation linear speed of the casting rolls is ≤0.8m / s. The present invention also provides a thin strip steel produced according to the above method.
[0007] In a preferred embodiment, the content of selenium (Se) is in the range of 0.005% to 0.01% by weight.
[0008] In a preferred embodiment, the temperature of the molten metal in the molten pool is in the range of 1550°C to 1570°C.
[0009] In a preferred embodiment, the wetting angle formed by the molten metal on the surface of the casting roll is less than 80°.
[0010] In a preferred embodiment, the molten metal in the molten pool also includes, by weight: no more than 0.03% carbon (C), no more than 0.5% silicon (Si), no more than 0.2% manganese (Mn), no more than 0.005% nitrogen (N), and no more than 0.005% sulfur (S).
[0011] The present invention also provides a thin strip steel produced by a twin-roll continuous casting machine, comprising by weight: no more than 0.03% carbon (C), no more than 0.5% silicon (Si), no more than 0.2% manganese (Mn), no more than 0.005% nitrogen (N), no more than 0.005% sulfur (S), and no less than 0.005% selenium (Se). Preferably, the content of selenium (Se) is in the range of 0.005% to 0.01% by weight. The selenium (Se) added to the thin strip steel enables, during the casting process, the molten steel to be cooled and solidified on the surface of the casting roll with an improved wetting angle, and the formed thin strip steel can be formed into a longer continuous length, and the strip thickness is uniform and the fluctuation is small.
[0012] The method of the present invention improves the wettability of thin strip continuous casting molten steel on the surface of the casting roll, specifically:
[0013] (1) The Se content in the molten steel is ≥0.005% by weight. Adding Se to the molten steel can effectively reduce the surface tension of the molten steel. The higher the Se content, the smaller the surface tension of the molten steel, the smaller the wetting angle of the molten steel on the surface of the casting roll, and the better the wettability. In order to make the wetting angle of the molten steel on the surface of the casting roll less than 90°, preferably less than 80°, the Se content in the present invention needs to be ≥0.005% by weight. However, considering the requirements for the purity of molten steel in this field, the Se content cannot be increased indefinitely, and is generally selected to be ≤0.01%.
[0014] (2) The molten steel flows into the molten pool through the tundish and the transition ladle, and the temperature of the molten steel in the molten pool is controlled to be ≥1550°C; the higher the temperature of the molten steel, the smaller the surface tension of the molten steel, the smaller the wetting angle of the molten steel on the surface of the casting roll, and the better the wettability. In order to make the wetting angle of the molten steel on the surface of the casting roll less than 90°, preferably less than 80°, the temperature of the molten steel is ≥1550°C. However, too high a temperature of the molten steel will directly result in the molten steel being unable to solidify into a strip on the surface of the casting roll. Therefore, the temperature of the molten steel generally does not exceed 1570°C.
[0015] (3) Control the linear speed of the casting rolls to be ≤0.8 m / s. The rotation of the casting rolls will affect the stability of the molten steel on the surface of the casting rolls, and thus affect the wettability. Generally, the slower the casting rolls move, the better the wettability of the molten steel on their surface. Therefore, the ideal state of the casting rolls is static. However, considering the requirements of the thin strip casting and rolling process, the casting rolls must rotate continuously to remove the steel strip from the molten pool. Therefore, the casting rolls cannot remain static. Taking all factors into consideration, the present invention controls the linear speed of the casting rolls to be ≤0.8 m / s.
[0016] According to a method of improving the wettability of the surface of a thin strip continuous casting casting roll by molten steel of the present invention, the wetting angle formed by the molten steel on the surface of the casting roll can be less than 90°, preferably less than 80°.
[0017] Beneficial technical effects
[0018] The method of the present invention can improve the wettability of the casting roller surface with molten steel during thin strip continuous casting, with the wetting angle being less than 90°, preferably less than 80°, so that the molten steel adheres better to the casting roller surface, cools evenly, solidifies into a strip that is stable and has uniform thickness, is less likely to break, thereby improving production continuity, improving product quality, and reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly introduce the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings of the embodiments. Obviously, the drawings in the following description only relate to some implementation cases of the present invention, and are not intended to limit the present invention.
[0020] Figure 1 is a schematic side view of a twin-roll continuous casting machine system of the present invention;
[0021] Figure 2 is through Figure 1 A partial cross-sectional view of the casting rolls installed in the roll box in the casting position of a twin-roll continuous caster. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one of ordinary skill in the art to which the present invention belongs.
[0024] The following are embodiments of the present invention. The described embodiments are only a part of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments that can be obtained by ordinary technicians in this field without making any creative work are within the scope of protection of the present invention.
[0025] Now refer to Figure 1 and Figure 2 , shows a twin-roll continuous casting machine, which includes a main frame 10, which stands upright from the floor and supports a pair of casting rolls 12, which are installed in a roll box 11 for easy operation and movement.
[0026] A twin roll continuous caster for continuously casting thin metal strip includes a pair of counter-rotating casting rolls 12, each having a casting surface 12A, with a nip 18 formed therebetween. Molten metal is transferred from a ladle 13 through a tundish 14, then through a refractory outlet shield 15 to a transitional ladle 16, and then to a distributor 17 positioned between the casting rolls 12 above the nip 18. The molten metal so transferred forms a molten pool 19 supported above the nip and above the casting surfaces 12A of the casting rolls 12.
[0027] The casting rolls 12 are internally cooled (e.g., water-cooled), so that as the casting rolls 12 rotate relative to each other, the molten metal in the molten pool 19 rotates in contact with the casting surface 12A and is cooled and solidified on the casting surface 12A. During the casting process, the metal shell formed by cooling and solidifying on the casting surface 12A of the casting rolls 12 is brought together at the nip 18 between the casting rolls to form a thin strip steel product that is transferred downward from the nip.
[0028] The twin-roll continuous casting machine is particularly suitable for manufacturing high-strength lightweight steel strip products and can achieve continuous and efficient production. In the technical solution of the present invention, in particular, adding non-metallic elements, such as selenium (Se), to the molten metal (molten steel) can improve the wettability of the molten metal (molten steel) on the casting roll surface during the thin strip continuous casting process.
[0029] Preferably, the amount of selenium (Se) added is selected so that, during the thin strip continuous casting process, the wetting angle of the molten steel on the surface of the casting roll is less than 90°, preferably less than 80°. The good wettability of the molten metal on the surface of the casting roll enables the molten metal to adhere well to the surface of the rotating casting roll and cool evenly, so that the steel strip formed by the cooling and solidification of the molten metal on the surface of the casting roll is continuous, stable and uniform in thickness, and is not prone to strip breakage, thereby improving production continuity and reducing production costs.
[0030] Adding Se element to molten steel can effectively reduce the surface tension of molten steel, and the higher the Se content, the smaller the surface tension of molten steel, and then the smaller the wetting angle of molten steel on the surface of casting roll, and the better the wettability. In the scenario of the present invention, wettability refers to the degree of wetting of liquid (molten steel) on solid surface (casting roll surface), wherein at the junction of solid, liquid and gas, the angle from solid-liquid interface through liquid interior to gas-liquid interface is called contact angle / wetting angle; wherein the smaller the wetting angle, the better the wettability. The most fundamental reason for wettability is the existence of liquid surface tension. Generally, the wetting angle of molten steel on the surface of casting roll less than 90°, preferably less than 80°, can achieve good wettability and fit, and thus continuous stability of casting during continuous casting, and uniform thickness of steel strip. Considering the requirements for surface tension and wettability of molten steel, as well as the requirements for purity of molten metal during continuous casting, the content of Se element is preferably selected from the range of about 0.005% to about 0.01%.
[0031] During the continuous casting of thin strip, the molten metal (molten steel) flows into the molten pool 19 through the tundish 14 and the transition ladle 16, wherein the molten pool 19 is formed above the roll gap 18 between the pair of relatively rotating casting rolls 12 and above the casting surface 12A. Increasing the temperature of the molten steel helps to reduce the surface tension of the molten steel, and the higher the temperature of the molten steel and the smaller the surface tension of the molten steel, the smaller the wetting angle of the molten steel on the surface of the casting roll, and the better the wettability. In order to keep the wetting angle of the molten steel on the surface of the casting roll less than 90°, preferably less than 80°, the temperature of the molten steel in the molten pool 19 is selected to be not less than 1550°C. At the same time, considering that the excessively high temperature of the molten steel will directly lead to the inability of the molten steel to quickly cool and solidify into a strip on the surface of the casting roll, the temperature of the molten steel is preferably selected to be not more than 1570°C.
[0032] After the molten metal flows into the molten pool 19, the casting roll 12 is internally cooled (e.g., water-cooled), so that as the casting roll 12 rotates relatively, the molten metal in the molten pool 19 continuously contacts the rotating casting roll surface 12A, and cools and solidifies on the casting surface 12A, thereby forming a thin strip steel product that is transmitted downward from the roll gap at the roll gap 18. The rotation speed of the casting roll will also affect the stability of the molten steel on the casting roll surface, thereby affecting the wettability. Generally, the slower the rotation of the casting roll, the better the wettability of the molten steel on its surface, and the better the thickness stability of the formed steel strip, so the ideal state of the casting roll is static. However, considering the process requirements of thin strip continuous casting, the pair of casting rolls 12 must rotate relatively continuously in order to take the steel strip away from the molten pool and transmit it downward from the roll gap, so the casting roll cannot remain static. Taking into account the wettability and casting speed, in the technical solution of the present invention, the rotation line speed of the casting roll is ≤0.8m / s. In the context of the present invention, the linear speed of rotation of the casting roll is the linear speed of the casting roll surface, that is, the product of the angular speed of the casting roll and the radius of the casting roll.
[0033] Table 1 below lists several comparative examples and embodiments to illustrate the effects of Se content in molten steel, molten steel temperature in the molten pool and linear speed of rotation of the casting roll on the molten steel wetting angle on the casting roll surface (i.e., the molten steel wetting property on the casting roll surface) in the thin strip continuous casting process. With comprehensive consideration of the above factors, it is possible to achieve better wetting property of molten steel on the casting roll surface (e.g., the wetting angle is less than 90°, preferably less than 80°), achieve stable production for a long time, reduce production costs, improve production efficiency, and meet the actual needs of industrial production.
[0034] Table 1 Process and steel wettability of comparative examples and embodiments
[0035]
[0036] Specifically, according to the experimental results in Table 1, it can be seen that as the Se content in the molten steel increases, the temperature of the molten steel in the molten pool increases, and the linear speed of rotation of the casting roll decreases, the wetting angle of the molten steel on the surface of the casting roll shows a decreasing trend. Preferably, a Se content of not less than 0.005% (including 0.005%) is added to the molten steel, so as to maintain good wettability of the molten steel on the surface of the casting roll. Further, the temperature of the molten steel in the molten pool is preferably not less than 1550°C (including 1550°C), and the linear speed of rotation of the casting roll is preferably not more than 0.8m / s, so that the wetting angle of the molten steel on the surface of the casting roll can be achieved to be less than 80°, further achieving good wettability and adhesion of the molten steel on the surface of the casting roll, and thus continuous stability of casting during continuous casting.
[0037] Furthermore, in the production process of the present invention, in addition to the selenium (Se) element, the molten metal also includes: no more than 0.03% carbon (C), no more than 0.5% silicon (Si), no more than 0.2% manganese (Mn), no more than 0.005% nitrogen (N), and no more than 0.005% sulfur (S). Furthermore, the present invention also provides a steel strip product formed according to the aforementioned improved production method of the present invention, comprising by weight: no more than 0.03% carbon (C), no more than 0.5% silicon (Si), no more than 0.2% manganese (Mn), no more than 0.005% nitrogen (N), no more than 0.005% sulfur (S), and no less than 0.005% selenium (Se). Preferably, the content of selenium (Se) is in the range of 0.005% to 0.01% by weight. As mentioned above, Se added to molten steel helps to improve the wettability of the molten steel on the surface of the casting rolls, thereby ensuring a longer continuous length of the produced steel strip and uniform thickness.
[0038] The above description is only a specific implementation of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for improving the wettability of molten steel on the surface of a thin strip continuous casting roll, comprising the following steps: The molten metal flows to a pair of casting rolls of a twin-roll continuous casting machine and forms a molten pool above the roll gap between the pair of casting rolls and above the casting surfaces of the casting rolls, wherein the temperature of the molten metal in the molten pool is in the range of 1560° C. to 1565° C., The molten metal in the molten pool also includes, by weight: Not more than 0.03% carbon (C), Not more than 0.5% silicon (Si), Not more than 0.2% of manganese (Mn), 0.005% to 0.008% selenium (Se), Not more than 0.005% nitrogen (N), Not more than 0.005% sulfur (S), The pair of casting rolls rotate relative to each other, and the molten metal in the molten pool cools and solidifies on the casting surfaces of the casting rolls and passes downward through the roll gap between the pair of casting rolls to form a steel strip, wherein the rotational linear speed of the casting rolls is ≤0.8 m / s, and the wetting angle formed by the molten metal on the surfaces of the casting rolls is less than 79.6°.
2. A thin steel strip produced according to the method of claim 1.
Citation Information
Patent Citations
Method for casting a composite ingot
CN102089101A
Fast heat treatment method for controlling magnetic property of double-roller thin-strip casting non-oriented silicon steel
CN104178617A
Preparation method for thin-strip continuous casting strong Goss texture Fe-Si alloy thin-strip billet
CN108179352A
Method for producing 30CrMo hot-rolled steel plate / strip through thin-strip continuous casting
CN112522581A
Metal casting
CN1136482A