A method for preparing copper-based powder metallurgy material for high-energy load braking conditions
Through the preparation method of copper-based powder metallurgical materials, combined with the ratio and process steps of copper powder, tin powder and other components, the problem that traditional materials are difficult to meet the high-energy braking conditions, and high wear resistance and anti-bonding are achieved , suitable for high-speed braking needs of high-speed trains.
Patent Information
- Application Number
- CN202211005245.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-08-22
AI Technical Summary
Traditional braking materials are difficult to meet the requirements of high-speed and lightweight development of high-speed railway EMUs, and cannot meet the performance requirements of friction materials under high-energy braking conditions.
Using the preparation method of copper-based powder metallurgical materials, by mixing, pressing, sintering and assembly by combining copper powder, tin powder, iron powder, graphite powder, ferroalloy powder, hard metal powder, ceramic particles and non-metallic carbides Steps to form a friction material with high wear resistance, adhesive resistance and noise reduction.
It realizes high wear resistance, adhesion resistance and noise reduction of materials under high-energy braking conditions, meeting the braking performance requirements of high-speed trains.
Smart Images

Figure CN115351272B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper-based friction materials, and more specifically to a method for preparing a copper-based powder metallurgy material for high-energy load braking conditions. Background Art
[0002] High-speed trains are developing in the direction of high speed, light weight and intelligence. The stable operating speed of high-speed trains has reached or exceeded 300km / h, and is developing towards higher speed. Under emergency braking conditions at 300km / h, the braking energy density is as high as 450J / mm2. During the braking process, the unit area energy load of the friction pair material is higher than 3000J / cm2, which is called high-energy braking. At the same time, high-energy braking makes the flash point temperature of the friction pair contact surface as high as 900℃. Therefore, traditional brake materials have been difficult to adapt to the development requirements of high-speed and lightweight trains. There is an urgent need for a preparation method of copper-based powder metallurgy materials for high-energy load braking conditions to meet the needs. Summary of the invention
[0003] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for preparing a copper-based powder metallurgy material for high-energy load braking conditions.
[0004] To achieve the above object, the present invention provides the following technical solution: a method for preparing a copper-based powder metallurgy material for high-energy load braking conditions, comprising the following steps:
[0005] S1. Material preparation stage: the raw materials of the friction body include copper powder, tin powder, iron powder, graphite powder, ferroalloy powder, hard metal powder, ceramic phase particles, and non-metallic carbide;
[0006] S2, mixing stage, mixing according to the ratio requirements, putting various weighed powder raw materials and an appropriate amount of organic solvent into a mixer to mix to obtain a uniform mixture;
[0007] S3, in the pressing stage, the mixture is weighed to a required weight, placed in a steel mold for pressing, and a holding time is set. After the pressing is completed, a compact of a desired shape is obtained;
[0008] S4, sintering stage, the green compacts are evenly placed on the tooling tray and stacked to a certain height, and placed in a sintering furnace with a protective atmosphere, and the insulation time is set. After the insulation time is completed, the green compacts are cooled and taken out of the furnace to obtain the desired sintered parts;
[0009] S5, in the assembly stage, the sintered parts are assembled and connected with the remaining parts to obtain the finished EMU brake pads.
[0010] The present invention is further configured as follows: in the step S1, the raw materials used for preparing the copper-based powder metallurgy friction material include the following components in terms of mass percentage: copper powder 40-55%, tin powder 1-4%, iron powder 10-20%, graphite powder 10-18%, ferroalloy powder 5-11%, hard metal powder 0.5-3%, ceramic particles 0.5-2.5%, and non-metallic carbide 0.5-2.5%.
[0011] The present invention is further configured as follows: the copper powder has a particle size range of 50-200 μm; the tin powder has a particle size range of 50-200 μm; the iron powder has a particle size range of 50-200 μm; the ferroalloy powder has a particle size range of 10-120 μm; the hard metal powder has a particle size range of 0-45 μm; the ceramic phase particles have a particle size range of 0-45 μm; and the non-metallic carbide has a particle size range of 0-45 μm.
[0012] The present invention is further configured as follows: the graphite powder includes granular graphite and flake graphite, the particle size range of the granular graphite is 60-300 μm; the particle size range of the flake graphite is 150-500 μm, and the mass ratio of the granular graphite to the flake graphite is 1:3-1:1.
[0013] The present invention is further configured as follows: the ferroalloy powder includes one or two of ferromolybdenum and ferrochromium.
[0014] The present invention is further configured as follows: the hard metal powder includes one or both of tungsten powder and molybdenum powder.
[0015] The present invention is further configured as follows: the ceramic phase particles include one or more of mullite, zirconium oxide, and zircon sand.
[0016] The present invention is further configured as follows: the non-metallic carbide particles include one or both of boron carbide and silicon carbide.
[0017] The present invention is further configured as follows: in step S3, the molding pressure is set to 200-400 MPa, and the holding time is set according to the actual situation, and after the pressing is completed, the compact of the desired shape is obtained.
[0018] The present invention is further configured as follows: in the step S4, the protective atmosphere is set to a mixed gas of nitrogen and hydrogen, the sintering temperature is set to 890-1000° C., and the holding time is set to 1.5-3 h.
[0019] By adopting the above technical scheme, in terms of material preparation ratio, the present invention mainly adopts copper powder as the matrix in the friction material formula, adds tin powder and copper powder to form a copper-tin alloy reinforcement matrix during the sintering process, adds an appropriate amount of iron powder with good compatibility with copper powder to enhance the strength of the friction material matrix, and can also adjust the friction coefficient and wear resistance, and adds hard metal powders such as tungsten and molybdenum. After sintering, tungsten and molybdenum are not dissolved in the matrix Cu, and mainly exist in the matrix in the form of particles, but tungsten and molybdenum have higher specific heat capacity and can absorb the heat generated during the friction process. At the same time, tungsten and molybdenum can improve the wear resistance of the friction material together with the iron alloy particles; a certain amount of flake graphite is matched to ensure that the friction unit formed by sintering has good anti-sticking In terms of bonding and wear resistance, a certain amount of granular graphite is added to ensure that the friction unit formed by sintering has good wear resistance and corrosion resistance. At the same time, graphite, as a friction reducer, plays a role in protecting the pair and reducing noise. At the same time, a certain proportion of friction regulator is added to the friction material formula, and its main component contains an appropriate amount of ferroalloy powder. This type of alloy powder has good bonding with the copper base and is not easy to peel off under high-speed and high-heat conditions. It has the function of strengthening the matrix components, and selecting the appropriate particle size can adjust the friction coefficient and reduce the pair wear. The friction regulator also contains a small amount of ceramic particles, non-metallic carbides, etc. to increase the friction coefficient of the friction material and has a certain anti-adhesion effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The present invention is a flow chart of a method for preparing a copper-based powder metallurgy material for high-energy load braking conditions. DETAILED DESCRIPTION
[0021] Reference Figure 1 The embodiment of the method for preparing the copper-based powder metallurgy material for high-energy load braking conditions of the present invention is further described.
[0022] For ease of explanation, spatial relative terms such as "upper", "lower", "left", "right" and the like are used in the embodiments to illustrate the relationship of one element or feature shown in the figure relative to another element or feature. It should be understood that, in addition to the orientation shown in the figure, the spatial terms are intended to include different orientations of the device in use or operation. For example, if the device in the figure is inverted, the element described as being "under" other elements or features will be positioned "on" other elements or features. Therefore, the exemplary term "under" can include both upper and lower orientations. The device can be positioned in other ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here can be interpreted accordingly.
[0023] Furthermore, relational terms such as “first” and “second” and the like are merely used to distinguish one component from another having the same name, but do not necessarily require or imply any such actual relationship or order between these components.
[0024] A method for preparing a copper-based powder metallurgy material for high-energy load braking conditions comprises the following steps:
[0025] S1. Material preparation stage: raw materials include copper powder, tin powder, iron powder, graphite powder, ferroalloy powder, hard metal powder, ceramic phase particles, and non-metallic carbide;
[0026] S2, mixing stage, mixing according to the ratio requirements, putting the weighed various powder raw materials and an appropriate amount of organic solvent into a mixer to mix to obtain a uniform mixture;
[0027] S3, in the pressing stage, the mixture is weighed to a required weight, placed in a steel mold for pressing, and a holding time is set. After the pressing is completed, a compact of a desired shape is obtained;
[0028] S4, sintering stage, the green compacts are evenly placed on the tooling tray and stacked to a certain height, and placed in a sintering furnace with a protective atmosphere, and the insulation time is set. After the insulation time is completed, the green compacts are cooled and taken out of the furnace to obtain the desired sintered parts;
[0029] S5, in the assembly stage, the sintered parts are assembled and connected with the remaining parts to obtain the finished EMU brake pads.
[0030] In step S1, the copper-based powder metallurgy material formula is based on copper, and the raw materials used for preparation include the following components in terms of mass percentage, wherein copper powder 40-55%, with a particle size range of 50-200μm; tin powder 1-4%, with a particle size range of 50-200μm; iron powder 10-20%, with a particle size range of 50-200μm; graphite powder 10-18%, graphite powder includes granular graphite and flake graphite, the granular graphite particle size range is 60-300μm, the flake graphite particle size range is 150-500μm, and the mass ratio of granular graphite to flake graphite is 1:3-1:1; ferroalloy powder 5-11%, with a particle size range of 10-120μm; hard metal powder 0.5-3%, with a particle size range of 0-45μm; ceramic particles 0.5-2.5%, with a particle size range of 0-45μm; non-metallic carbide 0.5 -2.5%, with a particle size range of 0-45μm; copper-based powder metallurgy materials are composed of four parts, including a matrix component that constitutes the skeleton of the matrix metal, a lubricating component and a friction modifier. Copper powder is the main component of the matrix component. Tin powder and copper powder are sintered to form a copper-tin alloy, which has the effect of strengthening the matrix; iron powder can be slightly soluble in copper powder, which can improve the strength of the matrix while adjusting the friction coefficient and wear resistance; graphite powder is used as a lubricating component to stabilize the friction coefficient, reduce the wear value, prevent the friction pair from sticking, and have anti-seizure properties; ferroalloy powder and hard metal particles are part of the friction modifier, which have good affinity with the matrix metal and are stored in the matrix to adjust the wear resistance and friction coefficient of the friction material, and at the same time improve the strength of the matrix. A small amount of ceramic particles and non-metallic carbides are added to the friction modifier to increase the friction coefficient and also have anti-sticking and anti-seizure effects.
[0031] In step S2, according to the following mass ratio, copper powder 40-55%, particle size range 50-200μm; tin powder 1-4%, particle size range 50-200μm; iron powder 10-20%, particle size range 50-200μm; graphite powder 10-18%, graphite powder includes granular graphite and flake graphite, granular graphite particle size range 60-300μm, flake graphite particle size range 150-500μm, and the mass ratio of granular graphite to flake graphite is The ratio of the raw materials to the raw materials is 1:3-1:1; ferroalloy powder 5-11%, particle size range 10-120μm; hard metal powder 0.5-3%, particle size range 0-45μm; ceramic particles 0.5-2.5%, particle size range 0-45μm; non-metallic carbide 0.5-2.5%, particle size range 0-45μm; and add an appropriate amount of organic solvent and put them into a mixer for mixing. After mixing for 5-8 hours, a uniform mixture can be obtained.
[0032] In step S3, the powder metallurgy friction layer mixture is weighed to a required weight, put into a steel mold and first scraped flat, and then a certain weight of the transition layer mixture is weighed. The transition layer mixture is mainly composed of 1-8% low melting point metal and a copper alloy matrix. The thickness of the transition layer is set to be no more than 1 mm. During the sintering process, the low melting point metal appears in a liquid phase, which improves the wettability between the contacting components to improve the bonding force between the powder metallurgy friction layer and the steel back plate. After the transition layer is scraped flat, it is pressed. Under the conditions of a molding pressure of 200-400MPa and room temperature, the pressure is maintained for 5-20 seconds. After the pressing is completed, a compact of the desired shape is obtained.
[0033] In step S4, each compact is combined with a steel back plate and evenly placed on a special tooling tray. Multiple tooling trays that have been placed are stacked to a certain height and placed in a sintering furnace with a protective atmosphere (nitrogen and hydrogen mixed gas). Under the conditions of a sintering temperature of 890-1000°C and a pressure per unit area of 1-5MPa, the insulation time is 1.5-3h, and then the compact is cooled to room temperature and taken out of the furnace to obtain the desired sintered part.
[0034] In step S5, a certain number of sintered parts are connected to the required parts by means of retaining springs, and a plurality of connected components are fixedly arranged on a large steel back to obtain a finished EMU brake pad.
[0035] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Common changes and substitutions made by those skilled in the art within the scope of the technical solution of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a copper-based powder metallurgy material for high-energy load braking conditions, It is characterized in that The following steps are involved: S1. Material preparation stage: raw materials include copper powder, tin powder, iron powder, graphite powder, ferroalloy powder, hard metal powder, ceramic phase particles, and non-metallic carbide; S2, mixing stage, mixing according to the ratio requirements, putting various weighed powder raw materials and an appropriate amount of organic solvent into a mixer to mix to obtain a uniform mixture; S3, in the pressing stage, the mixture is weighed to a required weight, placed in a steel mold for pressing, and a holding time is set. After the pressing is completed, a compact of a desired shape is obtained; S4, sintering stage, the green compacts are evenly placed on the tooling tray and stacked to a certain height, and placed in a sintering furnace with a protective atmosphere, and the insulation time is set. After the insulation time is completed, the green compacts are cooled and taken out of the furnace to obtain the desired sintered parts; S5, assembly stage, assembling and connecting the sintered parts with other parts to obtain the finished EMU brake pad; In the step S1, the raw materials used for preparing the copper-based powder metallurgy material include the following components in terms of mass percentage: copper powder 40-55%, tin powder 1-4%, iron powder 10-20%, graphite powder 10-18%, ferroalloy powder 5-11%, hard metal powder 0.5-3%, ceramic particles 0.5-2.5%, non-metallic carbide 0.5-2.5%, the copper powder particle size range is 50-200 μm; the tin powder particle size range is 50-200 μm; the iron powder particle size range is 10-200 μm; The particle size range of the ferroalloy powder is 50-200 μm; the particle size range of the ferroalloy powder is 10-120 μm; the particle size range of the hard metal powder is 0-45 μm; the particle size range of the ceramic phase particles is 0-45 μm; the particle size range of the non-metallic carbide is 0-45 μm, the graphite powder includes granular graphite and flake graphite, the particle size range of the granular graphite is 60-300 μm; the particle size range of the flake graphite is 150-500 μm, and the mass ratio of the granular graphite to the flake graphite is 1:3-1:1; In step S3, the molding pressure is set to 200-400 MPa, and the holding time is set according to the actual situation, and a compact of the desired shape is obtained after the pressing is completed; In the step S4, the protective atmosphere is set to a mixed gas of nitrogen and hydrogen, the sintering temperature is set to 890-1000° C., and the holding time is set to 1.5-3 hours.