A method for treating waste liquid from waste lithium batteries and its application

Through a non-strong acid treatment method, citric acid and polyaluminum sulfate and other additives are used for leaching and flocculation treatment of waste lithium batteries, which solves the problems of environmental pollution and high cost in the treatment of waste lithium batteries, and achieves low energy consumption, low cost and Efficient metal ion recovery.

CN115466842BActive Publication Date: 2024-10-29JINWEI ENVIRONMENTAL PROTECTION TECH (CHANGZHOU) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202111338537.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-12
Publication Date
2024-10-29
Estimated Expiration
2041-11-12

AI Technical Summary

Technical Problem

The existing technology may cause environmental pollution and high economic costs when disposing of used lithium batteries, and may produce harmful gases and equipment corrosion problems during the operation.

Method used

Using a treatment method that does not require strong acid, through the steps of discharge, dismantling, roasting, soaking, stirring and precipitation, using citric acid, glucose and other additives, combined with polymerized aluminum sulfate and sodium carbonate, environmentally friendly metal ion leaching and flocculation treatment are carried out. Reduce energy consumption and costs.

Benefits of technology

It achieves the treatment of waste lithium battery waste liquid with harmless substance emission, low energy consumption and low cost, improves the leaching efficiency and flocculation effect of metal ions, reduces the risk of equipment corrosion, and promotes the secondary recovery of precious metals.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a method for treating waste liquid from waste lithium batteries (IPC classification number: H01 / M1054), and in particular to a method for treating waste liquid from waste lithium batteries and its application. A method for treating waste liquid from waste lithium batteries, characterized in that it comprises the following steps: (1) discharging the waste lithium batteries; (2) disassembling, screening, roasting, screening, and grinding the discharged batteries to obtain positive electrode active powder; (3) adding the screened positive electrode active powder to an acid solution, soaking, and obtaining a first mixed solution; (4) adding a reducing agent to the first mixed solution and stirring evenly to obtain a second mixed solution; (5) adding sulfate to the second mixed solution; (6) adding a first precipitant, standing and filtering; adding a second precipitant to the filtrate, standing and filtering. The present invention does not require the use of strong acid, avoids existing safety issues, and reduces the need for equipment corrosion protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for treating waste liquid from waste lithium batteries (IPC classification number: H01 / M1054), and in particular to a method for treating waste liquid from waste lithium batteries and application thereof. Background Art

[0002] Used lithium-ion batteries contain not only the components of the original new batteries, but also new substances generated by side reactions inside the batteries. When used batteries are exposed to the air without being processed, they may explode, causing the electrolyte solvents, electrode materials, binders and diaphragms in the lithium batteries to enter the environment with a high probability, thus causing environmental pollution.

[0003] Patent application CN201810353215.X discloses a method for recovering lithium from waste lithium batteries, but in the process, inorganic acid HNO 3 Although leaching has achieved satisfactory results, secondary environmental pollution problems may occur during the operation, such as harmful gas (NOx) emissions. Patent application CN201810645996.X discloses a method for treating waste lithium battery positive electrode materials and a recycling process for waste lithium batteries. In the treatment process, the reducing agent H 2 O 2 It is an inorganic chemical reagent and has obvious disadvantages compared with biomass reducing agents. 2 O 2 The price of biomass reductant is higher than that of biomass reductant. Therefore, it will cause higher economic cost.

[0004] Therefore, the present invention provides a method according to the present invention that does not require the use of strong acid, avoids possible safety issues, and reduces the need for equipment corrosion protection. At the same time, the reaction can be carried out at normal temperature and pressure. In addition, it can greatly reduce processing costs, is environmentally friendly, has the lowest energy consumption, and the precious metals in the filter residue can also be recycled for secondary use. Summary of the invention

[0005] In order to solve the above problems, the first aspect of the present invention provides a method for treating waste liquid from waste lithium batteries, which comprises the following steps:

[0006] (1) Discharge waste lithium batteries;

[0007] (2) dismantling the discharged waste lithium batteries to obtain crushed materials, screening the crushed materials, recovering positive electrode materials, roasting, screening, and grinding the positive electrode materials to obtain positive electrode active powder;

[0008] (3) adding the screened positive electrode active powder to the acid solution and soaking it to obtain a first mixed solution;

[0009] (4) adding a reducing agent to the first mixed solution and stirring evenly to obtain a second mixed solution;

[0010] (5) adding sulfate to the second mixed solution;

[0011] (6) Add the first precipitant, let it stand and filter; add the second precipitant to the filtrate, let it stand and filter.

[0012] As a preferred solution, the waste lithium battery is selected from at least one of lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt oxide, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.

[0013] As a preferred solution, the calcination temperature is 500-700°C. The calcination temperature is 550-650°C.

[0014] As a preferred solution, the calcination time is 2 to 4 hours.

[0015] As a preferred solution, the average particle size of the positive electrode active powder is 400-500 meshes.

[0016] As a preferred solution, the acid solution is one or more of formic acid, oxalic acid, and citric acid.

[0017] As a preferred solution, the acid solution is a citric acid (CAS No.: 77-92-9) aqueous solution.

[0018] As a preferred solution, the mass concentration of the citric acid aqueous solution is 50% to 60%.

[0019] As a preferred solution, the liquid-to-solid volume mass ratio of the citric acid aqueous solution to the positive electrode active powder is 1: (5-10) mL / g.

[0020] As a preferred solution, the liquid-to-solid volume mass ratio of the citric acid aqueous solution to the positive electrode active powder is 1: (7-8) mL / g.

[0021] As a preferred solution, the soaking time is 70 to 90 minutes.

[0022] Citric acid is a leaching aid, which improves the leaching environment, increases the leaching speed, and reduces the generation of harmful substances. The applicant has found through a large number of experiments that the concentration of citric acid has a great influence on the leaching efficiency of metal ions such as cobalt and nickel, and unexpectedly found that when the concentration of citric acid is 5 mol / L, the leaching efficiency of cobalt and nickel is the best. The applicant speculates that the H ionized by citric acid +The active ingredients promote the leaching of metal ions, and the carboxyl groups themselves have a coordination effect. However, when the concentration of citric acid is too high, the leaching rate will decrease, which may be because the ionization of citric acid becomes weaker when the concentration is high. However, the leaching effect of citric acid system on lithium is not obvious.

[0023] As a preferred embodiment, the reducing agent is one or more of glucose, ethanol, sucrose and fructose.

[0024] As a preferred solution, the reducing agent is a mixture of ethanol and sucrose.

[0025] As a preferred solution, the weight ratio of ethanol to sucrose is 1:1.

[0026] As a preferred solution, the sulfate is one or more of polyaluminum sulfate and polyferric sulfate.

[0027] As a preferred solution, the weight ratio of the polyaluminum sulfate to the polyferric sulfate is (0.5-1):1.

[0028] As a preferred solution, the polyferric sulfate is purchased from the polyferric sulfate of Henan Kexing Water Treatment Materials Co., Ltd.; the polyaluminum sulfate is purchased from the polyaluminum sulfate of Henan Kexing Water Treatment Materials Co., Ltd.

[0029] The present application improves the flocculation effect and the stabilization effect of the flocs by limiting the weight ratio of polyaluminium sulfate and polyferric sulfate. The applicant speculates that the synergistic effect of polyaluminium sulfate, polyferric sulfate and the system can make the surface and interior of the flocs play a bonding and consolidation role, thereby helping to avoid the looseness of these flocs and improve their compactness. However, flocculants such as polyaluminium sulfate and polyferric sulfate can flocculate metal components such as cobalt and nickel in the cathode waste liquid of lithium-ion batteries. When polyaluminium sulfate forms flocs with carbon powder, cobalt and nickel metal components in the waste liquid, although the flocs formed are relatively large and are easily deposited at the bottom of the system for filtration and removal, these flocs are relatively loose and easy to break. Although the flocs formed by polyferric sulfate are relatively small, they are dense enough, have high density, and are also easy to settle.

[0030] As a preferred solution, the first precipitant is one or more of an aqueous solution of sodium carbonate, an aqueous solution of potassium carbonate, and an aqueous solution of ammonium carbonate.

[0031] As a preferred solution, the first precipitant is a sodium carbonate aqueous solution; the mass concentration of the sodium carbonate aqueous solution is 300-350 g / L; the amount of the sodium carbonate aqueous solution added is 50-55 mL of the sodium carbonate aqueous solution in 1 L of solution.

[0032] The present application limits the concentration and addition amount of sodium carbonate, effectively improving the complexation of flocs and the flocculation effect, while also reducing the amount of sulfate and reducing costs. The applicant speculates that with the addition of sodium carbonate, the concentration of hydroxide will also increase, which will help the complexation between metal ions and impurities. These complexes can be adsorbed on the surface of flocs, improve the surface activity of these flocs, and promote the mutual aggregation of multiple flocs, thereby accelerating the precipitation rate.

[0033] As a preferred solution, the second precipitant is an alcohol compound.

[0034] As a preferred solution, the alcohol compound is one or more of methanol, ethanol, n-butanol, and octanol. The alcohol substance is an ethanol aqueous solution; the mass concentration of the ethanol aqueous solution is 80-90%.

[0035] As a preferred solution, the weight ratio of the first precipitant to the second precipitant is 1:(2-3).

[0036] Beneficial effects:

[0037] 1. This application uses an inorganic acid, citric acid, which does not produce harmful substances and is environmentally friendly. It can also greatly reduce processing costs and energy consumption.

[0038] 2. This application limits the concentration of citric acid to ionize H + The leaching of metal ions is achieved, and the leaching efficiency of cobalt and lithium is improved.

[0039] 3. The present application limits the particle size of the positive electrode active powder, which is beneficial to the controllability of the process and avoids the occurrence of agglomeration during the operation process, thereby affecting the removal of organic metals in the filtrate.

[0040] 4. The present application improves the stabilization effect of the floccules while improving the flocculation effect by limiting the weight ratio of polyaluminium sulfate to polyferric sulfate.

[0041] 5. The present application limits the concentration and addition amount of sodium carbonate, thereby effectively improving the complexation of flocculants and improving the flocculation effect, while also reducing the amount of sulfate used and reducing costs. DETAILED DESCRIPTION

[0042] Example

[0043] Example 1

[0044] Embodiment 1 of the present invention provides a method for treating waste liquid from waste lithium batteries, which comprises the following steps:

[0045] (1) Discharge waste lithium batteries;

[0046] (2) Dismantling the used lithium batteries after discharge, screening the crushed materials, recovering the positive electrode materials, roasting, screening and grinding the positive electrode materials to obtain positive electrode active powder.

[0047] (3) adding the screened positive electrode active powder to the acid solution and soaking it to obtain a first mixed solution;

[0048] (4) adding a reducing agent to the first mixed solution and stirring evenly to obtain a second mixed solution;

[0049] (5) adding sulfate to the second mixed solution;

[0050] (6) Add the first precipitant, let it stand and filter; add the second precipitant to the filtrate, let it stand and filter.

[0051] In step (1) of this embodiment, the calcination temperature is 600° C. and the calcination time is 3 h.

[0052] The average particle size of the positive electrode active powder in this embodiment is 450 mesh.

[0053] The acid solution in this embodiment is a citric acid aqueous solution, and the mass concentration of the citric acid aqueous solution is 55%.

[0054] In the citric acid aqueous solution of this embodiment, the liquid-to-solid volume mass ratio of the positive electrode active powder is 1:8 mL / g.

[0055] In step (3) of this embodiment, the soaking time is 80 minutes.

[0056] The reducing agent in this embodiment is a mixture of ethanol and sucrose, wherein the weight ratio of the ethanol to the sucrose is 1:1.

[0057] The reducing agent in this embodiment is a mixture of polyaluminum sulfate and polyferric sulfate; the weight ratio of the polyaluminum sulfate to the polyferric sulfate is 0.7:1.

[0058] As a preferred solution, the polyferric sulfate is purchased from the polyferric sulfate of Henan Kexing Water Treatment Materials Co., Ltd.; the polyaluminum sulfate is purchased from the polyaluminum sulfate of Henan Kexing Water Treatment Materials Co., Ltd.

[0059] In this embodiment, the first precipitant is a sodium carbonate aqueous solution; the concentration of the sodium carbonate is 320 g / L; and the amount of sodium carbonate added is 52 mL / L.

[0060] The second precipitant in this embodiment is an ethanol aqueous solution; the mass concentration of the ethanol aqueous solution is 85%.

[0061] As a preferred solution, the weight ratio of sodium carbonate to ethanol is 1:2.

[0062] Example 2

[0063] The specific implementation of Example 2 is the same as that of Example 1, except that the mass concentration of the citric acid aqueous solution in Example 2 is 60%.

[0064] Example 3

[0065] The specific implementation of Example 3 is the same as that of Example 1; the difference is that the weight ratio of polyaluminum sulfate to polyferric sulfate in Example 3 is 1:1.

[0066] Comparative Example 1

[0067] The specific implementation of Comparative Example 1 is the same as that of Example 1; except that the addition amount of sodium carbonate in Comparative Example 1 is 80 mL / L.

[0068] Comparative Example 2

[0069] The specific implementation of Comparative Example 2 is the same as that of Example 1; the difference is that in Comparative Example 2, the sulfate is aluminum sulfate.

[0070] Comparative Example 3

[0071] The specific implementation of Comparative Example 3 is the same as that of Example 1; the difference is that the reducing agent in Comparative Example 3 is ethanol.

[0072] Performance Testing

[0073] (1) The filtrate components of Examples 1 to 3 and Comparative Examples 1 to 3 were analyzed, and the contents of Co, Ni and Li were determined by ICP-5000 plasma atomic emission spectrometer.

[0074] Performance test data:

[0075] Table 1 is an analysis of the filtrate components prepared in Examples 1 to 3 and Comparative Examples 1 to 3

[0076] Table 1

[0077] Co / % Ni / % Li / % Example 1 0.02 0.03 0.01 Example 2 0.04 0.06 0.04 Example 3 0.02 0.03 0.03 Comparative Example 1 0.2 0.4 0.09 Comparative Example 2 0.4 0.3 0.2 Comparative Example 3 0.2 0.1 0.4

Claims

1. A method for treating waste liquid from waste lithium batteries, characterized in that: It includes the following steps: (1) Discharge waste lithium batteries; (2) dismantling the discharged waste lithium battery to obtain crushed materials, screening the crushed materials, recovering the positive electrode materials, roasting, screening, and grinding the positive electrode materials to obtain positive electrode active powder; the roasting temperature is 600° C., and the roasting time is 3 hours. (3) adding the screened positive electrode active powder to an acid solution and soaking the mixture to obtain a first mixed solution; the acid solution is a citric acid aqueous solution having a mass concentration of 55% and a soaking time of 80 min; (4) adding a reducing agent to the first mixed solution and stirring the mixture to obtain a second mixed solution; the reducing agent is a mixture of ethanol and sucrose; the weight ratio of the ethanol to the sucrose is 1:1; (5) adding sulfate to the second mixed solution; the sulfate is polyaluminum sulfate and polyferric sulfate, and the weight ratio of the polyaluminum sulfate to the polyferric sulfate is (0.5-1):1, (6) adding a first precipitant, standing and filtering; adding a second precipitant to the filtrate, standing and filtering; the first precipitant is a sodium carbonate aqueous solution, the mass concentration of the sodium carbonate aqueous solution is 320 g / L, and the amount of the sodium carbonate aqueous solution added is 52 mL of the sodium carbonate aqueous solution added to 1 L of the solution; the second precipitant is an ethanol aqueous solution, the mass concentration of the ethanol water is 85%, and the weight ratio of the sodium carbonate to the ethanol is 1:2; The average particle size of the positive electrode active powder is 450 meshes.

2. An application of the method for treating waste liquid from waste lithium batteries according to claim 1, characterized in that: Application in recycling valuable metals in lithium batteries.

Citation Information

Patent Citations

  • Method for selectively recovering lithium from waste lithium batteries and preparing lithium carbonate

    CN108550939A

  • Method for treating waste lithium battery positive electrode material and process for recycling waste lithium battery

    CN108899603A

  • Waste lithium battery wet wire recovery method

    CN109868364A

  • Method for recovering valuable metal made of lithium battery cathode material by using saccharides and hydrogen peroxide

    CN111455177A

  • Treatment method and application of lithium battery cathode waste liquid

    CN111620423A