A repair welding method for reducing internal defects of magnesium-lithium alloy workpieces

By combining solid solution heat treatment in TIG welding of magnesium lithium alloy workpieces, the problems of lithium burnout and oxidation inclusion are solved, the mechanical properties and formability of the welded joints are improved, and efficient welding repair of magnesium lithium alloy workpieces is achieved.

CN115502521BActive Publication Date: 2024-11-05SHANGHAI JIAOTONG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211279620.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-08-18
Filing Date
2022-10-19
Publication Date
2024-11-05
Estimated Expiration
2042-10-19

AI Technical Summary

Technical Problem

Magnesium lithium alloy workpieces are prone to defects during casting, especially during TIG welding, which can easily cause lithium burning, oxidation inclusions, evaporation cracks, pores and other defects in the heat-affected zone, resulting in a decrease in the mechanical properties of the welded joints, limiting magnesium. The widespread application of lithium alloys.

Method used

Tungsten electrode argon arc welding (TIG welding) combined with solid solution heat treatment, control welding heat input by adjusting the wire diameter, welding current and argon protection gas flow, reduce the burn-out and oxidation of lithium elements, and improve welding through solid solution heat treatment Mechanical properties of the joint.

Benefits of technology

The high strength and good formability of the welds are achieved, the age softening during welding is avoided, the mechanical properties and welding quality of magnesium lithium alloy workpieces are improved, and the production cost and cycle are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115502521B_ABST
    Figure CN115502521B_ABST
Patent Text Reader

Abstract

The present invention discloses a repair welding method for reducing internal defects of a magnesium-lithium alloy workpiece, and the process parameters of the TIG repair welding step need to meet the following requirements: a welding wire diameter of 1 to 4 mm, a welding current of 40 to 160 A, and an argon shielding gas flow rate of 5 to 15 L / min. The heat-affected zone in the repair welding process of the magnesium-lithium alloy workpiece can be divided into a solid solution zone and an aging zone. The present invention performs a solid solution heat treatment on the magnesium-lithium alloy workpiece after the repair welding, which is beneficial to reducing the welding thermal stress existing in the welding process, and at the same time, the second phase in the aging zone is solid-dissolved in the matrix, so that the weldment as a whole is solid-solution strengthened, thereby avoiding aging softening caused during the welding process. The weld obtained by the welding process has excellent mechanical properties, especially high strength of the weld; the weld obtained by the welding process has good formability, neat appearance, and no deformation; in addition, the welding process is simple and easy to operate, convenient to operate, high in efficiency and low in cost; at the same time, there is no splashing residual material during the implementation of the welding process.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims priority to patent application filed on August 18, 2022 with application number 202210994635.2. Technical Field

[0002] The invention belongs to the technical field of welding, and particularly relates to a repair welding method for reducing internal defects of a magnesium-lithium alloy workpiece. Background Art

[0003] Magnesium-lithium alloy is the lightest metal structural material currently used in engineering applications, with a density of 1.35 to 1.65 g / cm 3 It is 20% to 30% lighter than standard magnesium alloy and is known as "ultra-light alloy". It has the advantages of strong cold and hot deformation ability, low anisotropy, good electromagnetic shielding performance, good electrical and thermal conductivity, good shock absorption performance, excellent cutting processability and weldability, etc. It has broad application prospects in aerospace, weapon equipment, 3C electronic products, racing cars and other fields.

[0004] Although magnesium-lithium alloy has many excellent properties, its application field is constantly expanding, and its demand is increasing year by year, it is very easy to produce defects in the casting process due to its special properties. This is an inevitable engineering problem that limits the wider application of magnesium-lithium alloy. Magnesium and lithium have high chemical activity and are easily oxidized and burned during the smelting process. During the solidification process, defects such as looseness, segregation, pores, inclusions, and cold shuts are prone to occur. These defects will seriously affect the quality of castings, reduce the mechanical properties of castings, and may become a source of cracks, causing the castings to break during use, which must be solved. Especially in the field of aerospace, many important structural parts use large magnesium-lithium alloy castings, such as aviation optoelectronic pods and accelerometer housings, which have achieved good weight reduction effects. However, such components have complex structures and have various special-shaped curved surfaces, inner cavity structures, and wall thickness mutations, which further reduce the first-time pass rate of casting magnesium-lithium alloys. In the face of the current low pass rate of casting magnesium-lithium alloys, in addition to taking process measures and strengthening process control during the casting process, welding repair of casting defects is also an important quality assurance measure. In addition, the structural damage of magnesium-lithium alloy workpieces during service can also be remanufactured through welding repair, reducing production costs and cycles. Therefore, the welding repair technology of magnesium-lithium alloy workpieces has become the key to the development of magnesium-lithium alloys.

[0005] Some scholars at home and abroad have conducted extensive research on magnesium alloys through welding methods such as stir friction welding, plasma arc welding, vacuum electron beam welding and tungsten inert gas welding (TIG). Compared with other welding methods, TIG welding technology has the advantages of flexible operation, high welding efficiency and strong welding adaptability. It has been widely used in the welding of ordinary magnesium alloys and has achieved good results. According to literature search, the experimental study on the microstructure and properties of LZ91 magnesium-lithium alloy TIG welding joint (Light Alloy Processing Technology, 2017, 45(01): 61-68) recorded that LZ91 alloy was welded by AC tungsten inert gas welding (TIG) process, and the welding material had good forming performance. However, during TIG welding, when the high-temperature TIG arc acts on the magnesium-lithium alloy with low melting and boiling points, it is easy to cause surface depression and reduce the bearing area of ​​the joint. At the same time, during the welding process, the welding is affected by the welding heat cycle, and because magnesium and lithium have strong chemical activity and are easily oxidized, the weld has serious lithium burn-out problems, and will introduce oxide inclusions, as well as evaporation cracks, pores and burn-through defects in the heat-affected zone. These defects will seriously deteriorate the strength and plasticity of the joint. These problems reduce the overall mechanical properties of the magnesium-lithium alloy welded joint and seriously affect the development of magnesium-lithium alloys. Summary of the invention

[0006] The present invention aims to solve the problem that defects are easily generated in magnesium-lithium alloy workpieces during the casting process and provides a repair welding method for reducing internal defects of magnesium-lithium alloy workpieces. The purpose is to solve the problem of poor performance of welded joints caused by factors such as lithium burning and easy introduction of oxide inclusions during repair welding using conventional TIG process.

[0007] The present invention discloses a repair welding method for reducing internal defects of a magnesium-lithium alloy workpiece, and the process parameters of the TIG repair welding step are as follows: a welding wire diameter of 1 to 4 mm, a welding current of 40 to 160 A, and an argon shielding gas flow rate of 5 to 15 L / min. The heat-affected zone in the repair welding process of the magnesium-lithium alloy workpiece can be divided into a solid solution zone and an aging zone. The present invention adopts a solid solution heat treatment to carry out a solid solution heat treatment on the magnesium-lithium alloy workpiece after the repair welding, which is beneficial to reducing the welding thermal stress existing in the welding process, and at the same time, the second phase in the aging zone is solid-dissolved in the matrix, so that the weldment as a whole is solid-solution strengthened, thereby avoiding aging softening caused during the welding process. The weld obtained by the welding process has excellent mechanical properties, especially high strength of the weld; the weld obtained by the welding process has good formability, neat appearance, and no deformation; in addition, the welding process is simple and easy to operate, convenient to operate, high in efficiency and low in cost; at the same time, there is no splashing residual material during the implementation of the welding process.

[0008] The objective of the present invention is achieved through the following technical solutions:

[0009] The present invention provides a repair welding method for reducing internal defects of a magnesium-lithium alloy workpiece. The repair welding method comprises the following steps: performing wire-filling repair welding on the workpiece to be repaired by tungsten inert gas welding (TIG welding); the process parameters of the TIG welding must meet the following requirements: a welding wire diameter of 1 to 4 mm, a welding current of 40 to 160 A, and a flow rate of a shielding gas of 5 to 15 L / min.

[0010] The present invention is a welding of filler wire under protective gas. If the diameter of the wire is too small, the filling effect of the wire is not good. After one welding, the groove is not effectively filled, and the weld may still have a depression. If multiple welding fillings are performed, more oxidation inclusions will be introduced, reducing the mechanical properties of the weld; if the diameter of the wire is too large, the melting of the wire requires a larger heat input, which requires a larger welding current. The larger the welding current, the more serious the oxidation. At the same time, the large direct wire needs to reduce the welding speed to ensure the melting of the wire. In addition, although the filling amount of the wire with a larger diameter is sufficient, it also causes a waste of material. The influence of the welding current on the weld is: if the welding current is too small, although the wire can be melted, the temperature of the substrate under the influence of welding heat is low. After the molten droplet of the wire reaches the substrate, the cooling speed is too fast, and the gas cannot escape in time, which will produce pores; if the welding current is too large, it will cause serious element burnout and collapse after welding. The function of argon shielding gas is to protect against oxidation during welding. If the flow rate of argon shielding gas is too small, the protection effect is insufficient and the oxidation phenomenon is still serious. If the flow rate of argon shielding gas is too large, although it can play a good protective role, it will cause serious waste of argon gas.

[0011] Preferably, the filler wire used for repair welding has the same composition as the workpiece to be repaired. The mass percentage of each component of the filler wire is: 6-14wt% Li, 2-7wt% Zn, 0.2-3% RE, and the balance is Mg and unavoidable impurities. The impurities include one or more of Fe, Si, Cu, and Ni, and the total impurity content is less than 0.02wt%. The rare earth elements include one or more of Yb, Gd, Dy, Er, Tb, and Ho.

[0012] Preferably, the protective gas is an inert gas, including one or more of helium, neon, argon, krypton, xenon, and radon. The protective gas is preferably argon. The purity of argon reaches 99.9%. However, inert gases such as nitrogen and carbon dioxide are not as effective as argon because magnesium and lithium in magnesium-lithium alloys are active elements and are easy to react with them.

[0013] In the present invention, the burning loss of lithium element during TIG welding of magnesium-lithium alloy is mainly due to the reaction of lithium element with oxygen to generate smoke and the evaporation before magnesium under high heat input conditions. In the present invention, pure argon is used as a shielding gas during welding. By setting a reasonable shielding gas flow rate, there is no visible smoke during welding. The pure argon shielding gas reduces or avoids the generation of smoke. By adjusting TIG process parameters such as arc current and welding speed, the heat input is controlled within a reasonable range, thereby reducing the burning loss of lithium element.

[0014] Preferably, the steps of the repair welding method are as follows:

[0015] S1. Perform wire-filling repair welding on the area to be repaired of the magnesium-lithium alloy workpiece by tungsten inert gas welding;

[0016] S2. Perform solid solution treatment on the repaired welded workpiece.

[0017] Preferably, in step S1, the shape of the area to be repaired is a semi-ellipse, and the semi-ellipse area smoothly transitions with the surface of the base material. Before welding, the area to be repaired and the surface of the welding wire are cleaned.

[0018] Preferably, in step S2, the solution temperature used for the solution treatment is 300-400°C and the time is 2-24h. The TIG welding process of magnesium-lithium alloy of the present invention benefits from the effect of grain refinement, and the obtained refined grain structure can improve welding strength and reduce the sensitivity of welding cracks; there is no obvious change in the grain size of the heat affected zone after welding. After solution heat treatment, the second phase particles are dissolved into the matrix, and the solid solution strengthening effect is obvious, thereby improving the mechanical properties of the welded joint. During TIG welding, the temperature of the liquid metal in the molten pool drops rapidly after welding, resulting in non-equilibrium solidification. The grains solidify before they have time to grow, thereby achieving the effect of grain refinement. The degree of grain refinement is related to the cooling rate. The higher the welding heat input, that is, the higher the current, the lower the cooling rate.

[0019] Preferably, the repair welding conditions are: the temperature is not lower than 0° C., the relative humidity is not higher than 85%, and no preheating is required during welding.

[0020] Preferably, the "front wire feeding" method is used for filling the welding wire during repair welding. There are two commonly used wire feeding methods: "front wire feeding" and "back wire feeding". Different wire feeding methods have different heating mechanisms for the welding wire. The "front wire feeding" method melts the welding wire more fully, the welding wire and the base metal are completely fused, and the weld performance is better.

[0021] Preferably, the area to be repaired is obtained by the following method:

[0022] A1. Detect internal defects of magnesium-lithium alloy workpieces by X-ray flaw detection method;

[0023] A2. Perform machining on the detected internal defects, dig out the defective parts, and form the groove to be repaired, that is, the area to be repaired.

[0024] There are two main reasons why TIG welding of magnesium-lithium alloys causes surface depressions: First, due to the low melting and boiling points of magnesium-lithium alloys, magnesium and lithium elements will evaporate or oxidize under the action of the high-temperature TIG arc, resulting in element burnout in the weld. In addition, when the welding current is too large, burn-through will occur, causing the unsolidified metal in the molten pool to sag. And in the present invention, the defective parts are repaired by welding, and grooves are processed in the repaired parts. Insufficient filling metal will also cause depressions. Therefore, homemade wires with the same composition are used, and the weld is filled with metal by the front wire feeding method during the TIG welding process to make up for the weld depression caused by metal loss in the weld, and a certain excess height will be formed in the weld after welding.

[0025] The welding heat cycle refers to the process in which the temperature of a certain point in the welding workpiece changes with time under the action of the heat source generated by the welding current. The welding heat cycle reflects the thermal effect of the welding heat source on the weld and the nearby metal, causing different changes in the organization and performance. For the welding of magnesium-lithium alloys, there is a problem of evaporation and oxidation at high temperature. The present invention adopts TIG welding under argon protection, and effectively controls the burning of elements by exploring suitable current parameters. In addition, under the action of the thermal cycle, a solid solution removal and aging zone are formed in the heat-affected zone. The present invention obtains a solid solution strengthening effect on the entire welded workpiece through subsequent heat treatment, thereby improving the mechanical properties of the workpiece. The oxidation problem will cause oxide inclusions in the weld. The presence of inclusions destroys the continuity of the metal body and reduces the strength and plasticity of the metal; the presence of inclusions is prone to cause stress concentration, significantly reducing the impact toughness and fatigue strength of the metal; when inclusions are distributed at the grain boundary, they not only reduce the strength but also cause thermal cracking; inclusions can also promote the formation of pores, which can adsorb gas and are a good substrate for the formation of gas nuclei.

[0026] Evaporation cracks in the heat-affected zone mainly occur at the junction with the weld. In the heat-affected zone near the weld, part of the metal melts and evaporates. During the cooling process, due to the contraction of the solidified metal and the presence of gas, insufficient residual liquid metal is generated, which causes stress during the cooling process, causing cracks in the liquid metal under the action of stress. In the present invention, evaporation cracks can be avoided by mainly allowing the gas to escape.

[0027] There are several main reasons for the formation of pores: too fast welding speed, too high welding current, moisture or oil on the surface of the welding workpiece or welding wire, etc. In the present invention, before TIG welding, the welding workpiece and the welding wire surface are cleaned, and welding is performed at a fixed welding speed and wire feeding speed with a reasonable welding current, so that the internal gas can escape easily. Burn-through is mainly caused by excessive current, and burn-through can be prevented by reducing the current.

[0028] In the present invention, the heat affected zone is divided into a solid solution zone and an aging zone, the solid solution zone is close to the weld, and the aging zone is far away from the weld. The formation of the solid solution zone is due to the solid solution of the AlLi phase under the action of high temperature, that is, the AlLi phase enters the matrix, which is beneficial to improve the performance of the workpiece; while the AlLi phase will precipitate in the aging zone, and the AlLi phase belongs to a softening phase, which will reduce the mechanical properties of the workpiece. In order to eliminate the influence of the aging zone, the workpiece is subjected to solid solution heat treatment after welding to promote the solid solution of the AlLi phase into the matrix, thereby improving the overall mechanical properties of the workpiece.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1) The weld obtained by the welding process has excellent mechanical properties, especially high strength of the weld; in addition, the weld obtained by the welding process has good formability, neat appearance, and no deformation; in addition, the welding process is simple and easy to operate, with high efficiency and low cost; at the same time, there is no spatter or residual material during the implementation of the welding process.

[0031] 2) The present invention adopts solution heat treatment to perform solution heat treatment on the workpiece after welding, so that the weldment as a whole is solid solution strengthened, thereby avoiding aging softening caused by the welding process.

[0032] 3) The present invention is beneficial to reducing the welding thermal stress existing in the welding process through post-welding solution heat treatment, which is beneficial to improving the uniformity of the welded workpiece and further improving the mechanical properties of the weldment.

[0033] 4) Tungsten inert gas welding of magnesium-lithium alloy is carried out under argon protection, which can effectively prevent the oxidation of magnesium-lithium alloy workpieces during welding. AC tungsten inert gas welding can play a "cathode breaking" role while obtaining a certain melting depth, removing the oxide inclusions on the surface of the workpiece. When the workpiece is the cathode, a large number of argon positive ions fly toward the workpiece at a very high speed and hit the surface of the workpiece. Since the positive ions are quite large and have great kinetic energy, the oxide film on the metal surface bombarded by the positive ions is broken, decomposed and evaporated, which plays a role in breaking and cleaning the oxide film on the surface of the weldment.

[0034] 5) The present invention repairs the defective part of the magnesium-lithium alloy workpiece by tungsten inert gas arc welding to obtain a magnesium-lithium alloy repaired workpiece without welding cracks, and can obtain a weld with a tensile strength equivalent to that of the base material, a weld with fine grains, and no obvious change in the grain size of the heat-affected zone. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0036] Figure 1It is a schematic diagram of the repair welding method of the present invention. DETAILED DESCRIPTION

[0037] The present invention is described in detail below in conjunction with embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0038] Example 1

[0039] This embodiment provides a repair welding method for reducing internal defects of a magnesium-lithium alloy workpiece. The repair welding method schematic diagram is shown in FIG. Figure 1 As shown, the specific steps are as follows:

[0040] The alloy composition of the workpiece to be welded and the filler wire is Mg-10Li-5Zn-0.5Er-0.2Yb (wt%, wt% refers to the percentage of the component in the total mass of the prepared magnesium-lithium alloy).

[0041] The area to be repaired of the magnesium-lithium alloy workpiece is repaired by tungsten inert gas welding, the diameter of the filling wire is 3mm, the welding current is 80A, and the flow rate of argon shielding gas is 10L / min;

[0042] The repaired workpiece was subjected to solution treatment at a temperature of 330°C and a solution time of 4 hours.

[0043] Under this welding condition, the performance test of the welded joint after solid solution treatment found that the tensile strength of the welding area reached 98% of the magnesium-lithium alloy workpiece body, and the elongation reached 95% of the magnesium-lithium alloy workpiece body.

[0044] Example 2

[0045] This embodiment provides a repair welding method for reducing internal defects of a magnesium-lithium alloy workpiece, and the specific steps are as follows:

[0046] The alloy composition of the workpiece to be welded and the filler wire is Mg-8Li-3Zn-0.2Y (wt%, wt% refers to the percentage of the component in the total mass of the prepared magnesium-lithium alloy).

[0047] The area to be repaired of the magnesium-lithium alloy workpiece is repaired by tungsten inert gas welding, the diameter of the filling wire is 3 mm, the welding current is 90 A, and the flow rate of argon shielding gas is 12 L / min;

[0048] The repaired workpiece was subjected to solution treatment at a temperature of 350°C and a solution time of 4 hours.

[0049] Under this welding condition, the performance of the welded joint after solution treatment was tested, and it was found that the tensile strength of the welding area reached 96% of the magnesium-lithium alloy workpiece body, and the elongation reached 98% of the magnesium-lithium alloy workpiece body.

[0050] Example 3

[0051] This embodiment provides a repair welding method for reducing internal defects of a magnesium-lithium alloy workpiece, and the specific steps are as follows:

[0052] The alloy composition of the workpiece to be welded and the filler wire is Mg-6Li-4Zn-1Gd (wt%, wt% refers to the percentage of the component in the total mass of the prepared magnesium-lithium alloy).

[0053] The area to be repaired of the magnesium-lithium alloy workpiece is repaired by tungsten inert gas welding, the diameter of the filling wire is 4 mm, the welding current is 120 A, and the flow rate of argon shielding gas is 14 L / min;

[0054] The repaired workpiece was subjected to solution treatment at a temperature of 300°C and a solution time of 6 hours.

[0055] Under this welding condition, the performance test of the welded joint after solid solution treatment found that the tensile strength of the welding area reached 97% of the magnesium-lithium alloy workpiece body, and the elongation reached 95% of the magnesium-lithium alloy workpiece body.

[0056] Comparative Example 1

[0057] A repair welding of a magnesium-lithium alloy workpiece, wherein the alloy composition is the same as that of Example 1, and the repair welding method of the alloy is basically the same as that of Example 1, except that the welding current for the repair welding of the alloy workpiece is 170A.

[0058] Under this welding condition, crystallization cracks appeared in some areas of the magnesium-lithium alloy workpiece after repair welding, and the oxide inclusions in the weld structure increased. Performance testing of the weld joint after welding showed that the tensile strength of the welding area reached 89% of the magnesium-lithium alloy workpiece body, and the elongation reached 87% of the magnesium-lithium alloy workpiece body.

[0059] When the welding current is too large, the heat input is too large, which is easy to cause thermal cracks. At the end of crystallization, there is a liquid film formed by low-melting eutectic (residual liquid phase). At this time, the metal plasticity is extremely low, and the tensile stress generated by the uneven contraction of cooling exceeds the tensile limit, which causes cracking.

[0060] Comparative Example 2

[0061] A repair welding method for a magnesium-lithium alloy workpiece, wherein the alloy composition and the repair welding method of the alloy are the same as those of Example 2, except that the alloy workpiece is not subjected to a solid solution treatment after the repair welding.

[0062] Under this welding condition, the performance test of the welded joint after welding found that the tensile strength of the welding area reached 87% of the casting body, and the elongation reached 90% of the casting body.

[0063] The weld microstructure of magnesium-lithium alloy after repair welding is divided into fusion zone, heat-affected zone and matrix zone. However, magnesium-lithium alloy will undergo two phenomena, solid solution and aging, at different temperatures. Therefore, the heat-affected zone can be divided into solid solution zone and aging zone along the area away from the weld. Solid solution treatment of the weld after welding will promote the solid solution of the second phase in the aging zone in the alloy into the crystal, forming a solid solution strengthening effect and improving the uniformity of the magnesium-lithium alloy workpiece. If solid solution heat treatment is not performed after welding, the tensile strength at the weld of the magnesium-lithium alloy workpiece is 20% lower than the tensile strength at the weld of the magnesium-lithium alloy workpiece after solid solution strengthening.

[0064] Comparative Example 3

[0065] A repair welding method for a magnesium-lithium alloy workpiece, wherein the alloy composition and the repair welding method of the alloy are the same as those of Example 2, except that the diameter of the filler wire used for the repair welding is 1 mm.

[0066] Under this welding condition, the magnesium-lithium alloy workpiece is repeatedly filled with welding to form the weld excess height. The performance test of the welded joint after welding found that the tensile strength of the welding area reached 88% of the magnesium-lithium alloy workpiece body, and the elongation reached 85% of the magnesium-lithium alloy workpiece body.

[0067] Since the filler wire used for repair welding of magnesium-lithium alloy workpieces has a small diameter, multiple fillings are required. However, during this process, defects such as oxide inclusions and holes are easily formed, thereby reducing the mechanical properties of the weld of the magnesium-lithium alloy workpiece.

[0068] Matters not covered by the present invention are known technologies.

[0069] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A repair welding method for reducing internal defects of a magnesium-lithium alloy workpiece, characterized in that: The repair welding method comprises the following steps: using tungsten inert gas arc welding to perform wire-filling repair welding on the workpiece to be repaired; the process parameters of the tungsten inert gas arc welding are: a welding wire diameter of 4 mm, a welding current of 120 to 160 A, and a flow rate of a shielding gas of 10 to 15 L / min; The steps of the repair welding method are specifically as follows: S1. Perform wire-filling repair welding on the area to be repaired of the magnesium-lithium alloy workpiece by tungsten inert gas welding; S2. Performing solid solution treatment on the repair welding workpiece; In step S2, the solution treatment adopts a solution temperature of 300 to 400° C. and a time of 2 to 24 hours.

2. The repair welding method according to claim 1, characterized in that: The filler wire used for repair welding has the same composition as the workpiece to be repaired.

3. The repair welding method according to claim 2, characterized in that: The mass percentages of the components of the filler welding wire are: 6-14wt% Li, 2-7wt% Zn, 0.2-3% RE, and the remainder is Mg and unavoidable impurities.

4. The repair welding method according to claim 1, characterized in that: The protective gas is an inert gas, including one or more of helium, neon, argon, krypton, xenon and radon.

5. The repair welding method according to claim 1, characterized in that: In step S1, the shape of the area to be repaired is a semi-ellipse, and the semi-ellipse area smoothly transitions to the surface of the base material.

6. The repair welding method according to claim 1, characterized in that: The conditions for repair welding are: temperature not lower than 0℃, relative humidity not higher than 85%, and no preheating is required during welding.

7. The repair welding method according to claim 1, characterized in that: When repairing welding, the welding wire is filled in by the "forward wire feeding" method.

8. The repair welding method according to claim 1, characterized in that: The area to be repaired is obtained by the following method: A1. Detect internal defects of magnesium-lithium alloy workpieces by X-ray flaw detection method; A2. Perform machining on the detected internal defects, dig out the defective parts, and form the groove to be repaired, that is, the area to be repaired.