Ultrasonic assisted plasma-arc composite atomization powder making equipment and powder making method
The ultrasonic-assisted plasma-arc composite atomization technology solves the problems of low powder particle size control efficiency and low fine powder formation rate in the plasma atomization method, and achieves adjustable powder particle size and high fine powder formation in the range of 0~300 μm. powder rate, suitable for the field of additive manufacturing.
Patent Information
- Application Number
- CN202211660902.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-23
AI Technical Summary
When the existing plasma atomization method is used to prepare high-performance spherical powder, the powder particle size control efficiency is low, the cost is high, and the fine powder yield is low, making it difficult to meet the demand for fine powder in the additive manufacturing field.
Ultrasonic-assisted plasma-arc composite atomization equipment is used to start an arc between two metal wires through an arc power supply, and a plasma arc and ultrasonic generator are combined to apply vibration on the conductive tip, using supersonic plasma jets and auxiliary atomization gas fines. It can liquefy metal droplets, achieve powder refinement and spheroidization, and control powder particle size.
It improves the control accuracy of powder particle size and the powdering rate of fine powder, and realizes the adjustable powder particle size in the range of 0~300μm. The equipment is simple and the cost is low, and it is suitable for the field of additive manufacturing.
Smart Images

Figure CN115740471B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder making, and in particular relates to an ultrasonic assisted plasma-arc composite atomization powder making device and a powder making method. Background Art
[0002] Spherical powder is an important raw material for additive manufacturing, powder metallurgy, injection molding, surface spraying and other preparation processes. Its composition, particle size, sphericity, hollow powder rate, etc. are key factors affecting the performance of the final component. Taking the field of powder additive as an example, the selection of additive powder is generally based on three factors: energy and heat source, powder supply method, product size and precision requirements. At present, the commonly used powder particle size range in the field of additive manufacturing is 15~53 μm (fine powder) and 53~150 μm (coarse powder).
[0003] The powder preparation methods mainly include water atomization, gas atomization, electrode induction melting atomization and plasma atomization, among which the powder prepared by plasma atomization has the advantages of high sphericity, high density, low porosity, low oxygen content and smooth surface, so this method plays an important role in the field of high-performance spherical powder. However, the plasma atomization method has problems such as coarse powder particle size, relatively high cost and low fine powder yield, which need to be solved urgently.
[0004] Comparative Patent 1: US5707419 "Method of production of metal and ceramic powders by plasma atomization", the patent proposes a plasma fuse atomization process method, the technology uses metal wire of specified size as raw material, feeds it into the atomization furnace at a specific rate through the wire feeding system, passes through the annular plasma torch heating device at the outlet, and is melted and atomized under the action of the focused plasma arc to finally obtain metal powder. The whole process is carried out in an argon atmosphere, the melting and atomization process is not interfered by foreign impurities, and the product purity is high. Since metal wire is used as the processing raw material, powder with a specific particle size distribution can be obtained by controlling the feed speed, which improves the quality stability of the powder. The low concentration of suspended particles can effectively prevent the formation of associated particles, so that the powder has good fluidity, which is very conducive to the preparation of high-purity, high-sphericity, and 10~300μm metal powder. This method only relies on plasma arc atomization of metal wire, and adjusts the powder particle size by controlling the feed speed of the metal wire. The efficiency is low and the control effect on the powder particle size is limited.
[0005] Comparative Patent 2: US6372298B1 "High deposition rate thermal spray using plasma transferred wire arc", the invention discloses a method of using a plasma gun to atomize a current-carrying wire at high speed, generating and establishing a high-speed plasma transfer wire arc between the cathode and the free end of the melting electrode, the energy of the plasma arc is sufficient to melt the free end of the melting electrode and atomize it into fine metal particles, and the particles are projected to the powder collection device at a speed of 5080-6350 mm / min. The plasma and arc are protected by high-speed and high-flow gas, so that they converge outside the intersection of the free end of the metal wire and the plasma arc, avoiding the direct impact of the shielding gas on the free end of the metal wire and promoting the projection of particles onto the target surface. The disadvantage of this method is that the airflow velocity around the plasma and arc is very high (600~800 L / min), and it is easy to obtain large-particle powder (powder in the range of 100~300μm accounts for 80%).
[0006] Comparative Patent 3: WO2011054113A1 “Methods and apparatuses for preparing spheroidal powders”, which proposes a method and apparatus for preparing spheroidal powders using plasma spraying, and proposes that the wire or rod is preheated to a temperature below the melting point before melting and atomizing, which can improve the production efficiency of spherical powders. The apparatus includes an inductor for preheating raw materials, equipment for melting and atomizing (including power sources for electric arc and plasma arc), and a special device for reducing the contact of sprayed powder with pollutants generated in the process. The disadvantage of the method is that the atomized material is heated in two stages by a non-transferred arc, which is less efficient than a transferred arc.
[0007] Comparative Patent 4: WO2019232612A1 "Method and apparatus for producing high purity spherical metallic powders at high production rates from one or two wires." This patent proposes a method for efficiently producing high purity spherical metal powders using one or two metal wires, the equipment of the method includes a hot plasma gun with a supersonic nozzle, a wire feeding system for continuously supplying one or two spray wires, and a special reactor for solidifying atomized particles into spherical powders. Two or more power supplies are used in parallel to control the arc between two metal wires or between a metal wire and a welding gun, and at least one power supply has a voltage / current control system. The metal wire is fed into the center of the plasma gun, an arc is generated in the supersonic nozzle and the metal wire is melted, and the plasma gun atomizes the molten metal wire into particles. After passing through the plasma gun, the molten particles enter the cooling chamber, and the atomized metal droplets pass through a diffuser, which is used to prevent the powder from recirculating, thereby preventing them from agglomerating, and finally the metal droplets solidify into spherical powders. The wire can be replaced by a rod with a diameter of 6.35 to 63.5 mm. The disadvantage of the method is that the powdering rate of fine powder is still difficult to ensure.
[0008] Improvements need to be made in view of the above technical problems. Summary of the invention
[0009] The present invention proposes a device for preparing powder using ultrasound-assisted plasma-arc composite atomization, and discloses a method for preparing powder using the device. The device and method disclosed in the present invention can adjust the powder particle size within the range of 0-300 μm according to demand, improve the fine powder formation rate, and have high powder preparation efficiency.
[0010] In order to achieve the above purpose, the technical scheme adopted by the present invention is: an ultrasonic assisted plasma-arc composite atomization powder making equipment, including an arc power supply, a plasma arc power supply, a first ultrasonic generator, a second ultrasonic generator, a first wire feeding device, a second wire feeding device, a plasma gun and an atomization chamber; the plasma gun includes a plasma cathode, a plasma gun water cooling nozzle, a plasma gas inlet and an auxiliary atomization gas inlet; the plasma cathode is placed in the center of the plasma gun, and the plasma gas inlet surrounded by the plasma gun water cooling nozzle is arranged on the periphery of the plasma gun water cooling nozzle. Auxiliary atomizing gas inlet; a first wire feeding device and a second wire feeding device are placed on both sides of the plasma gun, the first wire feeding device is used to convey the first metal wire to the first conductive nozzle, and the second wire feeding device is used to convey the second metal wire to the second conductive nozzle, the conveyed first metal wire and the second metal wire meet in front of the water-cooled nozzle of the plasma gun, and the first conductive nozzle, the second conductive nozzle and the front end of the plasma gun are all placed in the atomization chamber; the positive and negative poles of the arc power supply are respectively connected to the first conductive nozzle and the second conductive nozzle; the positive pole of the plasma arc power supply is connected to the water-cooled nozzle of the plasma gun, and the negative pole is connected to the plasma cathode.
[0011] As a preferred solution of the present invention, the first metal wire and the second metal wire are solid metal wires with a diameter of 0.6-3.0 mm.
[0012] As a preferred embodiment of the present invention, the first metal wire and the second metal wire are cored metal wires with a diameter of 1.6-5.0 mm.
[0013] As a preferred solution of the present invention, nanostructured metal oxides, carbides and silicides are added to the core of the cored metal wire.
[0014] A powder making method of an ultrasonic assisted plasma-arc composite atomization powder making device, the specific steps are as follows:
[0015] Step 1: Passing a first metal wire and a second metal wire of required powder material through a first conductive nozzle and a second conductive nozzle through a first wire feeding device and continuously feeding the wires during a subsequent arcing process;
[0016] Step 2: supplying plasma forming gas from the plasma gas inlet and supplying auxiliary atomizing gas from the auxiliary atomizing gas inlet;
[0017] Step 3: using an arc power source to start an arc between the first metal wire and the second metal wire, using a first ultrasonic generator to apply ultrasonic vibration to the first conductive nozzle, and using a second ultrasonic generator to apply ultrasonic vibration to the second conductive nozzle, so as to decompose the molten metal at the ends of the first metal wire and the second metal wire into;
[0018] Step 4: At the same time as step 3, a plasma arc power supply is used to start an arc between the water-cooled nozzle of the plasma gun and the plasma cathode, and a gas compression arc is formed through the plasma to generate a supersonic plasma jet;
[0019] Step 5: The metal droplets are further refined and accelerated under the action of the supersonic plasma jet and the auxiliary atomizing gas;
[0020] Step 6: The refined metal droplets pass through the atomization chamber, spheroidize and solidify, and the resulting powder is deposited at the bottom of the chamber.
[0021] As a preferred solution of the present invention, the wire feeding speed of the first wire feeding device and the second wire feeding device is 2-200 m / min.
[0022] As a preferred solution of the present invention, the arc power supply applies a rectangular pulse modulated current between the first metal wire and the second metal wire, with a current range of 0-600A, a frequency of 30-300Hz, and a voltage of 20-80V.
[0023] As a preferred solution of the present invention, the rectangular pulse modulation current is a bipolar pulse modulation, the minimum current intensity is 0-60A, and the ratio of the peak value to the minimum value is 10:1.
[0024] As a preferred embodiment of the present invention, the first ultrasonic generator and the second ultrasonic generator provide ultrasonic vibrations of 20-40 kHz and a power of 300-500 W.
[0025] As a preferred embodiment of the present invention, the plasma forming gas introduced from the plasma gas inlet is argon, helium, or a mixture of argon and helium, and the flow rate of the plasma forming gas is 100-300 L / min.
[0026] As a preferred embodiment of the present invention, the plasma arc power supply applies a current of 60-600A and a voltage of 100-250V between the water-cooled nozzle of the plasma gun and the plasma cathode, and applies a pulse modulation of 20-40kHz.
[0027] As a preferred embodiment of the present invention, the auxiliary atomizing gas introduced from the auxiliary atomizing gas inlet is oxygen or an argon-oxygen mixed gas, and the flow rate of the auxiliary atomizing gas is 5% to 20% of the flow rate of the plasma forming gas.
[0028] As a preferred solution of the present invention, the atomization chamber needs to be evacuated before powdering.
[0029] As a preferred solution of the present invention, the atomization chamber needs to be filled with inert protective gas before powder making.
[0030] As a preferred embodiment of the present invention, ultrasonic vibration is applied to one of the first conductive nozzle and the second conductive nozzle.
[0031] The beneficial effects of the present invention are:
[0032] 1. Use an arc power supply to start an arc between two metal wires, so that the ends of the metal wires melt and decompose into droplets. The droplets can be broken up and accelerated by using a supersonic plasma jet. The arc-plasma arc composite mode accelerates the melting and atomization process of the metal wires;
[0033] 2. By applying ultrasonic vibration to the wire feeding device, the molten metal droplets at the front end of the metal wire can be further broken up, thereby achieving the purpose of powder refinement. By adjusting the ultrasonic vibration frequency and power, the powder particle size can be controlled to a certain extent;
[0034] 3. Using an arc power supply, applying bipolar rectangular pulses to modulate the current between the wires can control the decomposition of the molten metal at the front end of the wire;
[0035] 4. Use one set of arc power supply to connect two wire feeding devices and start the arc between two metal wires, which not only saves energy, but also improves efficiency and makes the equipment simple and compact;
[0036] 5. Using the auxiliary atomizing gas inlet arranged on the periphery of the plasma gun to introduce oxygen, oxygen-argon mixed gas, etc. can promote the melting of the front ends of the two metal wires, improve the melting efficiency, and thus improve the powder making efficiency; in addition, the auxiliary atomizing gas can assist the plasma jet to switch to the injection mode, thereby achieving the effect of reducing the size of the atomized particles.
[0037] In summary, the ultrasonic-assisted plasma-arc composite atomization powder making equipment and powder making method proposed in the present invention are simple in equipment and low in cost. The powder making method controls and refines the powder particle size through a variety of means, thereby achieving adjustable powder particle size in the range of 0 to 300 μm. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is a schematic diagram of the principle of the ultrasonic assisted plasma-arc composite atomization powder making equipment of the present invention;
[0039] Figure 2 Schematic diagram of the appearance of the powder obtained by the powder making method of the present invention;
[0040] Reference numerals in the figure: arc power supply 1, plasma arc power supply 2, first ultrasonic generator 3, second ultrasonic generator 4, first wire feeding device 5, second wire feeding device 6, plasma gun 7, first metal wire 8, second metal wire 9, first conductive nozzle 10, second conductive nozzle 11, plasma cathode 12, plasma gun water-cooled nozzle 13, plasma gas inlet 14, auxiliary atomizing gas inlet 15, supersonic plasma jet 16, powder 17, atomization chamber 18. DETAILED DESCRIPTION
[0041] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0043] like Figure 1 As shown, an ultrasonic-assisted plasma-arc composite atomization powder making device includes an arc power supply 1, a plasma arc power supply 2, a first ultrasonic generator 3, a second ultrasonic generator 4, a first wire feeding device 5, a second wire feeding device 6, a plasma gun 7 and an atomization chamber 18; the plasma gun 7 includes a plasma cathode 12, a plasma gun water-cooling nozzle 13, a plasma gas inlet 14 and an auxiliary atomization gas inlet 15, the plasma cathode 12 is placed in the center of the plasma gun 7, and the plasma gas inlet 14 is surrounded by the plasma gun water-cooling nozzle 13, and an auxiliary atomization gas inlet 15 is arranged on the periphery of the plasma gun water-cooling nozzle 13. An air inlet 15; a first wire feeding device 5 and a second wire feeding device 6 are placed on both sides of a plasma gun 7, the first wire feeding device 5 feeds a first metal wire 8 through a first conductive nozzle 10; the second wire feeding device 6 feeds a second metal wire 9 through a second conductive nozzle 11, the first metal wire 8 and the second metal wire 9 delivered meet in front of a water-cooled nozzle 13 of a plasma gun, the first conductive nozzle 10, the second conductive nozzle 11 and the front end of the plasma gun 7 are all placed in an atomization chamber 18; the positive and negative electrodes of the arc power supply 1 are respectively connected to the first conductive nozzle 10 and the second conductive nozzle 11; the positive electrode of the plasma arc power supply 2 is connected to the water-cooled nozzle 13 of the plasma gun, and the negative electrode is connected to the plasma cathode 12.
[0044] A powder making method of an ultrasonic assisted plasma-arc composite atomization powder making device, the specific steps are as follows:
[0045] Step 1: Pass the first metal wire 8 and the second metal wire 9 of the required powder material through the first conductive nozzle 10 and the second conductive nozzle 11 through the first wire feeding device 5 and the second wire feeding device 6, and continue to feed the wires during the subsequent arcing process;
[0046] Step 2: Plasma forming gas is introduced from the plasma gas inlet 14, and auxiliary atomizing gas is introduced from the auxiliary atomizing gas inlet 15;
[0047] Step 3: using an arc power source 1 to start an arc between the first metal wire 8 and the second metal wire 9, using a first ultrasonic generator 3 to apply ultrasonic vibration to the first conductive nozzle 10, and using a second ultrasonic generator 4 to apply ultrasonic vibration to the second conductive nozzle 10, so as to decompose the molten metal at the ends of the first metal wire 8 and the second metal wire 9 into small droplets;
[0048] Step 4: At the same time as step 3, a plasma arc power supply 2 is used to start an arc between the plasma gun water-cooled nozzle 13 and the plasma cathode 12, and a gas compression arc is formed by plasma to generate a supersonic plasma jet 16;
[0049] Step 5: The metal droplets are further refined and accelerated under the action of the supersonic plasma jet 16 and the auxiliary atomizing gas;
[0050] Step 6: The refined metal droplets pass through the atomization chamber 18, spheroidize and solidify, and the resulting powder 17 is deposited at the bottom of the chamber 18.
[0051] Optionally, in some embodiments, the first metal wire 8 and the second metal wire 9 are solid metal wires with a diameter of 0.6-3.0 mm.
[0052] Optionally, in some embodiments, the first metal wire 8 and the second metal wire 9 are flux-cored metal wires with a diameter of 1.6-5.0 mm to which nanostructured metal oxides, carbides and silicides are added.
[0053] Optionally, in some embodiments, the wire feeding speed of the first wire feeding device 5 and the second wire feeding device 6 is 2~200m / min.
[0054] Optionally, in some embodiments, the arc power supply 1 applies a rectangular pulse modulated current between the first metal wire 8 and the second metal wire 9, with a current range of 0~600A, a frequency of 30~300Hz, and a voltage of 20~80V. The rectangular pulse modulated current is a bipolar pulse modulation with a minimum current intensity of 0~60A and a ratio of peak value to minimum value of 10:1.
[0055] Optionally, in some embodiments, the first ultrasonic generator 3 and the second ultrasonic generator 4 can provide ultrasonic vibrations of 20-40 kHz and a power of 300-500 W.
[0056] Optionally, in some embodiments, the plasma forming gas introduced from the plasma gas inlet 14 is argon, or helium, or a mixture of argon and helium, and the flow rate of the plasma forming gas is 100-300 L / min.
[0057] Optionally, in some embodiments, the plasma arc power supply 2 applies a current of 60-600A and a voltage of 100-250V between the plasma gun water-cooled nozzle 13 and the plasma cathode 12, and applies a pulse modulation of 20-40kHz.
[0058] Optionally, in some embodiments, the auxiliary atomizing gas introduced from the auxiliary atomizing gas inlet 15 is oxygen or an argon-oxygen mixed gas, and the flow rate of the auxiliary atomizing gas is 5% to 20% of the flow rate of the plasma forming gas.
[0059] Optionally, in some embodiments, the atomization chamber 18 needs to be evacuated before powdering.
[0060] Optionally, in some embodiments, the atomization chamber 18 needs to be filled with an inert protective gas before powder making.
[0061] Optionally, in some embodiments, ultrasonic vibration may be applied to one of the first conductive nozzle (10) and the second conductive nozzle (11).
[0062] A specific test example is listed below to illustrate the powder making process and powder yield of the present invention.
[0063] Embodiment 1:
[0064] Industrial pure titanium TA-1 with a diameter of Ø1.6 mm was used as the solid metal wire; argon was used as the plasma forming gas with a flow rate of 120 L / min, and oxygen was used as the auxiliary atomizing gas (oxygen) with a flow rate of 12 L / min; the arc power supply current was rectangular pulse modulation current, the current range was 20~200 A, the voltage was 40 V, and the rectangular pulse modulation frequency was 200 Hz; the plasma power supply current was 400 A, the voltage was 200 V; the ultrasonic generator vibration frequency was 25 kHz, and the power was 350 W.
[0065] Using the above parameters, the industrial pure titanium TA-1 powder obtained by the equipment and method proposed in the present invention has a powder yield of 82% for powders with a particle size of 0-100 μm.
[0066] Embodiment 2:
[0067] A flux-cored wire with a diameter of Ø3.0 mm was used. The main components of the flux-cored wire were 0.18% C + 1.5% Cr + 1.5% Mn + 0.8% Si + 0.6% Mo. The powder making process parameters were the same as those in Experimental Example 1.
[0068] Using the above parameters, the yield of 0-100 μm particle size powder obtained by the device and method proposed in the present invention is 79%.
[0069] The ultrasonic assisted plasma-arc composite atomization powder making equipment and powder making method proposed in the present invention have simple equipment and low cost. The powder making method controls and refines the powder particle size through various means, thereby achieving adjustable powder particle size within the range of 0-300 μm, especially within the particle size range of 0-100 μm. The powder yield is very high, so this method is very suitable for powder making in the field of additive manufacturing.
[0070] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention; therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
[0071] Although this article uses more of the figure markings: arc power supply 1, plasma arc power supply 2, first ultrasonic generator 3, second ultrasonic generator 4, first wire feeding device 5, second wire feeding device 6, plasma gun 7, first metal wire 8, second metal wire 9, first conductive nozzle 10, second conductive nozzle 11, plasma cathode 12, plasma gun water cooling nozzle 13, plasma gas inlet 14, auxiliary atomizing gas inlet 15, supersonic plasma jet 16, powder 17, atomization chamber 18 and other terms, it does not exclude the possibility of using other terms; these terms are used only to more conveniently describe and explain the essence of the present invention; interpreting them as any additional limitations is contrary to the spirit of the present invention.
Claims
1. An ultrasonic assisted plasma-arc composite atomization powder making equipment, characterized in that: The invention comprises an arc power supply (1), a plasma arc power supply (2), a first ultrasonic generator (3), a second ultrasonic generator (4), a first wire feeding device (5), a second wire feeding device (6), a plasma gun (7) and an atomizing chamber (18); the first ultrasonic generator (3) and the second ultrasonic generator (4) provide 20 to 40 kHz and a power of 300 to 500W ultrasonic vibration; the plasma gun (7) comprises a plasma cathode (12), a plasma gun water-cooling nozzle (13), a plasma gas inlet (14) and an auxiliary atomizing gas inlet (15); the plasma cathode (12) is placed in the center of the plasma gun (7), and the plasma gas inlet (14) is surrounded by the plasma gun water-cooling nozzle (13); the auxiliary atomizing gas inlet (15) is arranged on the periphery of the plasma gun water-cooling nozzle (13); a first wire feeding device (5) and a second wire feeding device (6) are placed on both sides of the plasma gun (7); the first wire feeding device (5) is used to feed a first metal wire (8) into a first conductive nozzle (10); the second wire feeding device (6) is used to feed a second metal wire (9) into a second conductive nozzle (11); the fed first metal wire (8) and the second metal wire (9) meet in front of the plasma gun water-cooling nozzle (13); the first wire feeding device (5) and the second wire feeding device (6 ... The front end of the electric nozzle (10), the second conductive nozzle (11) and the plasma gun (7) are all placed in an atomization chamber (18); the positive and negative electrodes of the arc power supply (1) are respectively connected to the first conductive nozzle (10) and the second conductive nozzle (11); the positive electrode of the plasma arc power supply (2) is connected to the plasma gun water-cooling nozzle (13), and the negative electrode is connected to the plasma cathode (12); the first metal wire (8) and the second metal wire (9) are cored metal wires with a diameter of 1.6 to 5.0 mm; nanostructured metal oxides, carbides and silicides are added to the cores of the cored metal wires; the arc power supply (1) applies a rectangular pulse modulated current between the first metal wire (8) and the second metal wire (9), the current range is 0 to 600 A, the frequency is 30 to 300 Hz, the voltage is 20 to 80 V, the rectangular pulse modulated current is bipolar pulse modulation, the minimum current intensity is 0 to 60 A, and the ratio of the peak value to the minimum value is 10:
1.
2. The ultrasonic assisted plasma-arc composite atomization powder making equipment according to claim 1, characterized in that: The first metal wire (8) and the second metal wire (9) are solid metal wires with a diameter of 0.6 to 3.0 mm.
3. A powder making method of the ultrasonic assisted plasma-arc composite atomization powder making equipment according to any one of claims 1 to 2, characterized in that: The specific steps are as follows: Step 1: A first metal wire (8) and a second metal wire (9) of required powder material are passed through a first conductive nozzle (10) and a second conductive nozzle (11) by a first wire feeding device (5) and a second wire feeding device (6), and the wires are continuously fed during a subsequent arcing process; Step 2: introducing plasma forming gas from the plasma gas inlet (14) and introducing auxiliary atomizing gas from the auxiliary atomizing gas inlet (15); Step 3: using an arc power source (1) to strike an arc between the first metal wire (8) and the second metal wire (9), using a first ultrasonic generator (3) to apply ultrasonic vibration to the first conductive nozzle (10), and using a second ultrasonic generator (4) to apply ultrasonic vibration to the second conductive nozzle (11), so as to decompose the molten metal at the ends of the first metal wire (8) and the second metal wire (9) into; Step 4: Simultaneously with step 3, a plasma arc power supply (2) is used to start an arc between a plasma gun water-cooled nozzle (13) and a plasma cathode (12), and a gas compression arc is formed by plasma to generate a supersonic plasma jet (16); Step 5: The metal droplets are further refined and accelerated under the action of the supersonic plasma jet (16) and the auxiliary atomizing gas; Step 6: The refined metal droplets pass through the atomization chamber (18), spheroidize and solidify, and the resulting powder (17) is deposited at the bottom of the atomization chamber (18).
4. The powder making method of the ultrasonic assisted plasma-arc composite atomization powder making equipment according to claim 3 is characterized in that: The wire feeding speeds of the first wire feeding device (5) and the second wire feeding device (6) are 2-200 m / min.
5. The powder making method of the ultrasonic assisted plasma-arc composite atomization powder making equipment according to claim 3, characterized in that: The arc power supply (1) applies a rectangular pulse modulated current between the first metal wire (8) and the second metal wire (9), with a current range of 0 to 600 A, a frequency of 30 to 300 Hz, and a voltage of 20 to 80 V.
6. The powder making method of the ultrasonic assisted plasma-arc composite atomization powder making equipment according to claim 5, characterized in that: The rectangular pulse modulated current is a bipolar pulse modulation with a minimum current intensity of 0~60A and a peak to minimum value ratio of 10:
1.
7. The powder making method of the ultrasonic assisted plasma-arc composite atomization powder making equipment according to claim 3, characterized in that: The first ultrasonic generator (3) and the second ultrasonic generator (4) provide ultrasonic vibrations with a frequency of 20 to 40 kHz and a power of 300 to 500 W.
8. The powder making method of the ultrasonic assisted plasma-arc composite atomization powder making equipment according to claim 3, characterized in that: The plasma forming gas introduced from the plasma gas inlet (14) is argon, helium, or a mixture of argon and helium, and the flow rate of the plasma forming gas is 100-300 L / min.
9. The powder making method of the ultrasonic assisted plasma-arc composite atomization powder making equipment according to claim 3, characterized in that: The plasma arc power supply (2) applies a current of 60 to 600 A and a voltage of 100 to 250 V between the plasma gun water-cooled nozzle (13) and the plasma cathode (12), and applies a pulse modulation of 20 to 40 kHz.
10. The powder making method of the ultrasonic assisted plasma-arc composite atomization powder making equipment according to claim 3, characterized in that: The auxiliary atomizing gas introduced from the auxiliary atomizing gas inlet (15) is oxygen or argon-oxygen mixed gas, and the flow rate of the auxiliary atomizing gas is 5% to 20% of the flow rate of the plasma forming gas.
11. The powder making method of the ultrasonic assisted plasma-arc composite atomization powder making equipment according to claim 3, characterized in that: Before powder making, the atomization chamber (18) needs to be evacuated.
12. The powder making method of the ultrasonic assisted plasma-arc composite atomization powder making equipment according to claim 3, characterized in that: Before powder making, the atomization chamber (18) needs to be filled with inert protective gas.
13. The powder making method of the ultrasonic assisted plasma-arc composite atomization powder making equipment according to claim 3, characterized in that: Ultrasonic vibration is applied to one of the first conductive nozzle (10) and the second conductive nozzle (11).