A method for preparing an outsourcing type drug-loaded visible nanofiber artificial vascular stent
The outer-type drug-loaded nanofiber vascular stent prepared by coaxial electrospinning technology solves the problems of immune response and unstable drug release rate of the internally implanted stent, achieves sustained release and real-time monitoring of drugs, and enhances vascular compatibility It has good properties and therapeutic effect and is suitable for the treatment of diseases such as macrovascular disease and myocardial infarction.
Patent Information
- Application Number
- CN202310044283.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-01-30
AI Technical Summary
Existing implantable vascular stents are easily recognized as foreign bodies by the immune system when implanted in the body, leading to immune reactions and thrombosis, and the sustained release rate of drugs is unstable, making it difficult to effectively treat primary lesions of large blood vessels, acute myocardial infarction and other diseases, and The toxicity and performance of fluorescent probes are insufficient to achieve real-time drug tracking.
Coaxial electrospinning technology is used to prepare an outer-type drug-loaded nanofiber artificial vascular stent. It is constructed in a layer-by-layer self-supporting manner and wrapped with carbon dots to achieve sustained drug release and real-time visual monitoring. The fluorescence properties of carbon dots are used to track the drug release rate. Enhance the compatibility between the stent and blood vessels.
It effectively prevents stent damage to the vascular intima, enhances biocompatibility, allows drugs to act directly on the affected area, reduces side effects, and improves therapeutic effects. It also monitors drug release in real time through carbon dot fluorescence imaging and adjusts medical plans.
Smart Images

Figure CN116036387B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of vascular stents, and in particular relates to a method for preparing an outsourced drug-loaded visible nanofiber artificial vascular stent. Background Art
[0002] Cardiovascular disease (CVD) is one of the leading causes of death worldwide. This project intends to study nanofiber-coated vascular stents, which are very different from traditional internal vascular stents. At present, most stents are internal implant stents, and their structural basis is bare metal stents. However, the tissue incompatibility of bare metal stents themselves leads to long-term irritation to the affected area, especially problems such as insufficient surface treatment that damage the smooth structure of the inner wall of the blood vessel. At the same time, the inflammatory response stimulates endothelial cells, leading to restenosis and stent thrombosis, and the related postoperative recovery problems are still prominent. To solve this problem, drug-eluting stents came into being. Drug-eluting stents use bare metal stents as their structural basis, and are attached with coatings and sustained-release drugs with good biocompatibility, which reduce irritation to the blood vessel wall while inhibiting the proliferation of intimal fibroblasts. However, the existing internal implant stents are easily recognized as foreign bodies by the immune system when implanted in the body, producing a strong immune response (such as adsorption of immunoglobulins, etc.), resulting in stent-like immune responses and thrombosis.
[0003] To this end, the form of outsourcing vascular stents is adopted, which can effectively prevent the stent from damaging the vascular endothelium and enhance the physical compatibility and biocompatibility between the stent and the blood vessel; then, by implanting drug nanofibers and continuously releasing drugs in situ, the immune response at the stent implantation site can be suppressed; in addition, the nanofiber tube is composed of layers of nanofiber blankets with excellent elasticity, and has a certain self-supporting strength, which can be completely convenient for the implantation process of the stent implantation device. However, the outsourcing stent has a relatively limited effect on the primary lesions of large blood vessels other than small blood vessel lesions, opening lesions, bifurcation lesions, chronic occlusive lesions, severe calcified lesions, and acute myocardial infarction lesions that require mechanical forced dilation of blood vessels. It is more suitable for postoperative drug administration and prevention of restenosis after open blood vessel surgery, intimal hyperplasia (IH), or arterial vascular transplantation for dialysis. Only by selecting a professional interventional team through professional judgment and operation can it achieve the best therapeutic effect.
[0004] In the out-wrapped vascular stent, the stent material wrapped around the blood vessel releases drugs. The sustained-release drugs are mainly targeted at the wrapped site for treatment, but they cannot be prevented from being lost to the surrounding tissues. The sustained-release rate of drugs in the body is often affected by multiple factors and is often different from the theoretical value of in vitro tests. Therefore, it is necessary to monitor carbon dots with fluorescence visualization to adjust the medical plan in a timely manner. Bioimaging technology can directly visualize biological patterns in real time and non-invasively through probes and detectors. As an imaging method, fluorescence imaging has become a powerful clinical diagnostic method due to its convenience, low cost, high sensitivity, non-invasiveness and long-term observation. However, conventional fluorophores such as traditional quantum dots (QDs) and organic dyes are plagued by toxicity issues or poor fluorescence properties, which has stimulated the rapid development of carbon dots (CDs). Carbon dots have excellent photostability, good biocompatibility, simple and fast synthesis, flexible designability, multi-color emission, deep red / NIR emission and two-light / multi-photon photoluminescence (PL), making CDs the next generation of fluorescent probes for in vitro and in vivo bioimaging. In addition to in vitro imaging, CDs with red / NIR emission or two-photon / multiphoton photoluminescence (PL) are excellent candidates for in vivo fluorescent tracking agents, taking advantage of the minimal autofluorescence and light scattering of tissues, providing excellent imaging contrast and spatial resolution, which provides a new approach for the prevention and treatment of brain diseases through real-time tracking. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing an out-wrapped drug-loaded visible nanofiber artificial vascular stent, which utilizes coaxial electrospinning technology to prepare drug-loaded nanofibers wrapped with carbon dots, and is constructed in a layer-by-layer self-supporting manner, which can flexibly control the diameter, wall thickness, drug loading, release rate, and visualize drug tracking, and can be applied to clinical artificial vascular stents.
[0006] To achieve the above object, the present invention is implemented through the following technical solutions:
[0007] A method for preparing an out-wrapped drug-loaded visible nanofiber artificial vascular stent comprises the following steps:
[0008] 1) Preparation of grape skin-based carbon dots
[0009] The grape skin powder is mixed with urea, heated at 190-220°C for 6-10 hours, cooled to room temperature, and the black product is ultrasonically dissolved in deionized water, centrifuged, and the collected supernatant is dialyzed through a dialysis membrane for 48-72 hours, and vacuum freeze-dried;
[0010] 2) Preparation of inner layer spinning solution containing carbon dots
[0011] Dissolve one or more of PEO, silk fibroin, and chitosan in water, acetic acid, or ether to obtain a polymer solution, and then add grape skin-based carbon dots;
[0012] 3) Preparation of drug-loaded outer spinning solution
[0013] Dissolving one of PI, PCL, PLGA, PLA, and PU in one or more of DMF, DCM, or HFIP containing baicalin;
[0014] 4) using the carbon dot-containing inner spinning solution prepared in step 2) as the core and the drug-loaded outer spinning solution prepared in step 2) as the shell to prepare a nanofiber membrane by a coaxial conjugate electrospinning method; the outer layer flow rate is 10 to 15 times that of the inner layer flow rate;
[0015] 5) using a rod-shaped mold with a diameter of 1 to 6 mm, rolling the nanofiber membrane obtained in step 4) into a nanofiber tube with a desired wall thickness, and drying at room temperature;
[0016] 6) Wrapping the nanofiber tubes prepared in step 5) around the affected blood vessels, fixing them via the connection sites, and releasing the drugs through the self-supporting shaping of the blood vessels by the nanofiber tubes.
[0017] In the preparation method of the grape skin powder described in step 1), the grape skin is ultrasonically cleaned with deionized water and alcohol for more than two times, dried and ground into powder.
[0018] In step 1), the mass ratio of grape skin powder to urea is 1:(2-3).
[0019] In the PEO solution described in step 2), the mass concentration of PEO is 10% to 18%.
[0020] The mass concentration of the grape skin-based carbon dots in the PEO solution in step 2) is 0.1% to 0.5%.
[0021] The mass concentration of baicalin in the drug-loaded outer spinning solution in step 3) is 1% to 5%.
[0022] In step 3), one of PI, PCL, PLGA, PLA, and PU is dissolved in one or more of DMF, DCM, or HFIP to prepare a PI or PCL, PLGA, PLA, or PU solution with a concentration of 15% to 20%.
[0023] In step 1), the vacuum freeze drying is performed at a temperature of -20 to -40°C.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The present invention wraps zero-dimensional structured photoluminescent carbon dots in the hollow core structure of the shaft shell mesoporous nanofibers by coaxial electrospinning, and finally forms a nanofiber membrane with good morphology, which is used to prepare an outwrapped vascular stent. The specific advantages are:
[0026] 1. The drug-loaded vascular stent wrapped with carbon dots prepared by the present invention can effectively prevent the stent from damaging the vascular endothelium and enhance the physical compatibility and biocompatibility between the stent and the blood vessel;
[0027] 2. By implanting drug nanofibers and continuously releasing the drug in situ, the drug can act directly on the affected area, solving the problems of baicalin, such as poor stability, poor lipid solubility and water solubility, low oral bioavailability, and difficulty in passing through the blood-brain barrier.
[0028] 3. The carbon dots located in the hollow core of mesoporous nanofibers play a vital role in "visualizing" the drug release rate and minimizing the side effects of the drug.
[0029] 4. Carbon dots CDs have advantages in visualizing drug accumulation and activity at pathological sites through their fluorescence properties, which plays an invaluable role in evaluating the therapeutic effects of drugs.
[0030] 5. The preparation method is simple and reliable, and the cost of preparation materials is low, and it can be applied to industrial preparation processes and clinical medicine. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 Schematic diagram of the electrospinning coaxial nanofiber device;
[0032] Figure 2 This is a scanning electron microscope image of the carbon-dot-loaded PI-PEO coaxial nanofiber membrane prepared in Example 1;
[0033] Figure 3 This is a fluorescence microscope image of the carbon-dot-loaded PI-PEO coaxial nanofiber membrane prepared in Example 1.
[0034] Figure 1 In the figure, 1- syringe one, 2- syringe two, 3- coaxial spinneret, 4- receiver. DETAILED DESCRIPTION
[0035] The present invention is described in detail below in conjunction with the accompanying drawings, but it should be noted that the implementation of the present invention is not limited to the following embodiments.
[0036] Using baicalin as a template drug, we intend to prepare hollow carbon dot-wrapped nanoporous fibers with good biocompatibility, and use them as drug-loaded nanofiber tubes for vascular stent implantation. Baicalin molecules leave the carrier and contact the carbon dots attached to the hollow inner core of the mesoporous nanofibers. The carbon dot fluorescence imaging "visualizes" the drug release rate in real time, and develop a type of baicalin fluorescence visual drug delivery system. The drug release site and release amount are detected by carbon dot fluorescence, achieving the clinical monitoring purpose of real-time monitoring and timely adjustment of medical plans.
[0037] Specifically, the preparation method of the externally-packaged drug-loaded visible nanofiber artificial vascular stent comprises the following steps:
[0038] 1) Preparation of grape skin-based carbon dots
[0039] Grape skin powder and urea are mixed in a mass ratio of 1:(2-3), heated at 190-220°C for 6-10 hours, cooled to room temperature, and the black product is ultrasonically dissolved in deionized water, centrifuged, and the collected supernatant is dialyzed for 48-72 hours, and vacuum freeze-dried;
[0040] The preparation method of grape skin powder comprises the following steps: washing the grape skin with deionized water and alcohol ultrasonically for more than two times, drying and grinding the grape skin into powder to obtain grape skin-based carbon dots.
[0041] 2) Preparation of inner layer spinning solution containing carbon dots
[0042] One or more of PEO, silk fibroin and chitosan are dissolved in water, acetic acid or ether to obtain a PEO solution with a PEO mass concentration of 10% to 18%, and grape skin-based carbon dots are added with a mass concentration of 0.1% to 0.5% of the PEO solution.
[0043] 3) Preparation of drug-loaded outer spinning solution
[0044] Dissolve one of soluble PI (polyimide), PCL (polycaprolactone), PLGA (polylactic acid-co-glycolic acid), PLA (polylactic acid), and PU (polyurethane) in one or more of DMF, DCM, or HFIP to prepare a PI or PCL, PLGA, PLA, or PU solution with a mass concentration of 15% to 20%, and then add baicalin thereto to obtain a drug-loaded outer layer spinning solution. The mass concentration of baicalin in the drug-loaded outer layer spinning solution is 1% to 5%.
[0045] The inner spinning of the carbon dots uses a solution that is insoluble in the drug-loaded outer spinning, so that coaxial nanofibers can be prepared. Otherwise, if the solution of the inner structure and the solution of the outer structure are easily miscible, the Taylor cone cannot be separated when high pressure is formed, and the nanofibers do not form a coaxial conjugated structure. PEO and silk fibroin with core structures are often used as carriers for sustained drug release because of their good biocompatibility and degradability. At the same time, the polymers used in the shell structure solution have good biocompatibility, but are not easy to degrade, and can exist in the body for a long time, so that the mechanical properties will not decrease after long-term use.
[0046] 4) The nanofiber membrane is prepared by a coaxial conjugate electrospinning method using the carbon dot-containing inner spinning solution prepared in step 2) as the core and the drug-loaded outer spinning solution prepared in step 2) as the shell; the outer layer flow rate is 10 to 15 times that of the inner layer flow rate.
[0047] See Figure 1 The electrospinning coaxial nanofiber equipment includes a syringe 1 (with an inner core solution conduit), a syringe 2 (with an outer shell solution conduit), a coaxial spinneret, and a roller receiver. The coaxial spinneret is a hollow double tube with an inner and outer concentric circle structure. The injection port of syringe 1 is connected to the inner tube of the coaxial spinneret, and the injection port of syringe 2 is connected to the outer tube of the coaxial spinneret. The receiver is used to collect the coaxial nanofibers. The inner diameter of the inner tube is 0.2-0.3 mm, the inner wall diameter of the outer tube is 0.8-1.2 mm, the voltage is 7kV-25kV, the distance between the needle and the receiving roller is 10-30 cm, the roller speed is 100-150rpm, and a nanofiber membrane is formed on the roller receiver. Figure 2 , Figure 3 , the inner spinning solution forms a core structure, and the outer spinning solution forms a shell structure.
[0048] When preparing the nanofiber membrane, the inner spinning solution containing the drug-loaded silver ions and the outer spinning solution are filled into the second syringe, and the inner spinning solution containing the drug-loaded silver ions and the outer spinning solution are injected into the outer tube of the coaxial spinneret, and the formed nanofiber membrane is collected by the receiver.
[0049] 5) Remove the nanofiber membrane and cut it to the required length and width. Use a rod-shaped mold with a diameter of 1 to 6 mm, which is a stainless steel rod with a PDMS (polydimethylsiloxane) layer on the outer shell, to roll the nanofiber membrane into a nanofiber tube with the required wall thickness without sealing it, that is, the cross-section of the nanofiber tube is an arc shape, and dry it at room temperature for more than 24 hours.
[0050] 6) Wrap the nanofiber tubes prepared in step 5) around the affected blood vessels in a bandage-like manner, fix them through the connection sites (biodegradable microneedles (MN)), and shape the blood vessels through the self-supporting layers of nanofiber tubes to release drugs, visualize drug tracking, and prevent blood vessel atrophy.
[0051] [Example 1]
[0052] The method for preparing an externally-packaged drug-loaded visible nanofiber artificial vascular stent comprises the following steps:
[0053] 1) Preparation of grape skin-based carbon dots. Grape skin was ultrasonically cleaned twice with deionized water and alcohol, then dried and ground into powder. 2.0 g of grape skin powder and 4.0 g of urea were mixed and transferred to a 50 mL crucible, then heated at 200 ° C for 8 hours and cooled to room temperature. The black product was ultrasonically dissolved in 20 mL of deionized water and centrifuged at 10000 rpm for 20 minutes to remove insoluble and larger particles. The collected supernatant was dialyzed with a dialysis membrane (MWCO 500) for 48 hours to remove unreacted raw materials and other impurities. Finally, after vacuum freeze drying at 50 ° C for 48 hours, grape skin-based carbon dots were obtained.
[0054] 2) Prepare the inner layer spinning solution containing carbon dots, dissolve PEO in water or ether with a mass concentration of 18%, add grape skin-based carbon dots fluorescent sensor for drug detection in an amount of 0.5% of the solution mass, and obtain the inner layer spinning solution containing carbon dots.
[0055] 3) preparing a drug-loaded outer spinning solution, dissolving soluble PI powder in a DMF solution, using baicalin as a drug source, and adjusting the mass percentage of baicalin in the solution to 1% to 5%;
[0056] 4) Use Figure 1 The electrospinning coaxial nanofiber device shown is used to manufacture nanofiber membranes, and the length and width are cut as needed; a rod-shaped mold with a diameter of 1 to 6 mm is used, and the rod-shaped mold is a stainless steel rod with a PDMS (polydimethylsiloxane) layer on the outer cover. The nanofiber membrane is rolled into a nanofiber tube with the required wall thickness for later use; the nanofiber tube is not sealed, that is, the cross-section of the nanofiber tube is an arc shape, and is dried at room temperature for more than 24 hours.
[0057] 5) According to actual clinical needs, the nanofiber tube is wrapped around the affected area in a bandage-like manner and fixed by biodegradable microneedles (MN) as connection sites. The nanofiber membrane is used to self-support and shape the blood vessels layer by layer, thereby achieving the triple effects of drug release, drug visualization and tracking, and preventing vascular atrophy.
[0058] [Example 2]
[0059] The method for preparing an externally-packaged drug-loaded visible nanofiber artificial vascular stent comprises the following steps:
[0060] 1) Grape skin-based carbon dots were prepared using the same process as in Example 1.
[0061] 2) PEO is dissolved in water or ether to obtain a PEO solution, wherein the mass concentration of PEO is 10%, and grape skin-based carbon dots are added to the PEO solution to obtain an inner layer spinning solution containing carbon dots, wherein the amount of grape skin-based carbon dots accounts for 0.5% of the mass of the solution.
[0062] 3) PCL was dissolved in a mixed solution of DCM and DMF to obtain a PCL solution with a mass concentration of 10%, the mass ratio of DCM to DMF in the mixed solution was 4:6, and baicalin was added as a drug source, and the mass percentage of baicalin in the PCL solution was 1% to 5%.
[0063] 4) Use Figure 1 The electrospinning coaxial nanofiber device shown is used to manufacture nanofiber membranes, and the length and width are cut as needed; a rod-shaped mold with a diameter of 1 to 6 mm is used, and the rod-shaped mold is a stainless steel rod with a PDMS (polydimethylsiloxane) layer on the outer cover. The nanofiber membrane is rolled into a nanofiber tube with a required wall thickness for standby use; the nanofiber tube is not sealed, that is, the cross-section of the nanofiber tube is an arc shape, and is dried at room temperature for more than 24 hours.
[0064] 5) According to actual clinical needs, the nanofiber tube is wrapped around the affected area in a bandage-like manner, fixed by biodegradable microneedles (MN) as connection sites, and the nanofiber membrane is used to self-support and shape the blood vessels, thereby playing the triple role of releasing drugs, visually tracking drugs, and preventing vascular atrophy.
[0065] [Example 3]
[0066] The method for preparing an externally-packaged drug-loaded visible nanofiber artificial vascular stent comprises the following steps:
[0067] 1) Grape skin-based carbon dots were prepared using the same process as in Example 1.
[0068] 2) Prepare the inner spinning solution containing carbon dots, dissolve PEO in water or ether at a mass concentration of 15%, add grape skin-based carbon dots fluorescent sensor for drug detection at an amount of 0.3% of the solution mass, and obtain the inner spinning solution containing carbon dots.
[0069] 3) PU is dissolved in HFIP to obtain a PU solution with a mass concentration of 20%, and baicalin is added as a drug source, and the mass percentage of baicalin in the PU solution is 1% to 5%.
[0070] 4) Use Figure 1The electrospinning coaxial nanofiber device shown is used to manufacture nanofiber membranes, and the length and width are cut as needed; a rod-shaped mold with a diameter of 1 to 6 mm is used, and the rod-shaped mold is a stainless steel rod with a PDMS (polydimethylsiloxane) layer on the outer cover. The nanofiber membrane is rolled into a nanofiber tube with a required wall thickness for standby use; the nanofiber tube is not sealed, that is, the cross-section of the nanofiber tube is an arc shape, and is dried at room temperature for more than 24 hours.
[0071] 5) According to actual clinical needs, the nanofiber tube is wrapped around the affected area in a bandage-like manner and fixed with biodegradable microneedles (MN) as the connection site. The nanofiber membrane is used to self-support and shape the blood vessels layer by layer, thereby achieving the triple effects of drug release, drug visualization and tracking, and preventing vascular atrophy.
[0072] [Example 4]
[0073] The method for preparing an externally-packaged drug-loaded visible nanofiber artificial vascular stent comprises the following steps:
[0074] 1) Grape skin-based carbon dots were prepared using the same process as in Example 1.
[0075] 2) preparing a carbon dot inner layer spinning solution, dissolving silk fibroin in acetic acid at a mass concentration of 18%, adding a grape skin-based carbon dot fluorescent sensor for drug detection at an amount of 0.3-0.5% of the solution mass, and obtaining a carbon dot inner layer spinning solution.
[0076] 3) PCL was dissolved in a mixed solution of DCM and DMF to obtain a PCL solution with a mass concentration of 10%, the mass ratio of DCM to DMF in the mixed solution was 4:6, and baicalin was added as a drug source, and the mass percentage of baicalin in the PCL solution was 1% to 5%.
[0077] 4) Use Figure 1 The electrospinning coaxial nanofiber device shown is used to manufacture nanofiber membranes, and the length and width are cut as needed; a rod-shaped mold with a diameter of 1 to 6 mm is used, and the rod-shaped mold is a stainless steel rod with a PDMS (polydimethylsiloxane) layer on the outer cover. The nanofiber membrane is rolled into a nanofiber tube with a required wall thickness for standby use; the nanofiber tube is not sealed, that is, the cross-section of the nanofiber tube is an arc shape, and is dried at room temperature for more than 24 hours.
[0078] 5) According to actual clinical needs, the nanofiber tube is wrapped around the affected area in a bandage-like manner and fixed by biodegradable microneedles (MN) as connection sites. The nanofiber membrane is used to self-support and shape the blood vessels layer by layer, thereby achieving the triple effects of drug release, drug visualization and tracking, and preventing vascular atrophy.
[0079] [Example 5]
[0080] The difference from Example 4 is that the carbon dot inner layer spinning solution is prepared differently, specifically:
[0081] Prepare the inner spinning solution containing carbon dots, dissolve chitosan in acetic acid with a mass concentration of 20%, add grape skin-based carbon dots fluorescent sensor for drug detection with an amount of 0.3-0.5% of the solution mass, and obtain the inner spinning solution containing carbon dots.
Claims
1. A method for preparing an out-wrapped drug-loaded visible nanofiber artificial vascular stent, characterized in that: The following steps are involved: 1) Preparation of grape skin-based carbon dots The grape skin powder is mixed with urea, heated at 190-220°C for 6-10 hours, cooled to room temperature, and the black product is ultrasonically dissolved in deionized water, centrifuged, and the collected supernatant is dialyzed with a dialysis membrane for 48-72 hours, and vacuum freeze-dried; 2) Preparation of inner layer spinning solution containing carbon dots Dissolve PEO in water to obtain a PEO solution, wherein the mass concentration of PEO is 10% to 18%, and then add grape skin-based carbon dots, wherein the mass concentration of the grape skin-based carbon dots in the PEO solution is 0.1% to 0.5%; 3) Preparation of drug-loaded outer layer spinning solution Dissolving one of soluble PI, PCL, PLGA, PLA, and PU in one or more of DMF, DCM, or HFIP to prepare a PI, PCL, PLGA, PLA, or PU solution with a mass concentration of 15% to 20%, and then adding baicalin thereto to obtain a drug-loaded outer layer spinning solution; the mass concentration of baicalin in the drug-loaded outer layer spinning solution is 1% to 5%; 4) using the carbon dot-containing inner spinning solution prepared in step 2) as the core and the drug-loaded outer spinning solution prepared in step 3) as the shell to prepare a nanofiber membrane by a coaxial conjugate electrospinning method; the outer layer flow rate is 10 to 15 times that of the inner layer flow rate; 5) Using a rod-shaped mold with a diameter of 1 to 6 mm, the nanofiber membrane obtained in step 4) is rolled into a nanofiber tube with a desired wall thickness and dried at room temperature.
2. The method for preparing an out-wrapped drug-loaded visible nanofiber artificial vascular stent according to claim 1, characterized in that: In the preparation method of the grape skin powder described in step 1), the grape skin is ultrasonically cleaned with deionized water and alcohol for more than two times, dried and ground into powder.
3. The method for preparing an out-wrapped drug-loaded visible nanofiber artificial vascular stent according to claim 1, characterized in that: In step 1), grape skin powder and urea are mixed in a mass ratio of 1:(2-3).
4. The method for preparing an out-wrapped drug-loaded visible nanofiber artificial vascular stent according to claim 1, characterized in that: In step 1), the vacuum freeze drying is carried out at a temperature of -20 to -40°C.
Citation Information
Patent Citations
Preparing device and method for forming micro-nanofiber
CN104451912A
Carbon quantum dot / fibroin composite nanofiber and preparing method and application thereof
CN109853068A
Self-anticoagulation developable small-caliber artificial intravascular stent and preparation method thereof
CN111632206A
External vascular stent and application thereof
CN111760179A