A kind of electropolymer gel electrolyte battery and preparation method thereof
The polymer network gel is formed in the gel electrolyte battery through electrochemical in-situ polymerization technology, which solves the problems of complex process and poor interface compatibility in the existing technology, realizes high-performance and simplified process battery preparation, and is suitable for a variety of Application scenarios.
Patent Information
- Application Number
- CN202310127663.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-14
AI Technical Summary
The preparation process of existing gel electrolyte batteries is cumbersome and requires a large amount of organic solvents, which leads to environmental pollution. In addition, the interface compatibility between gel electrolytes and electrodes is poor, affecting battery performance.
The electrochemical method is used to polymerize the gel electrolyte in situ in the battery, and the precursor solution of anionic polymer monomer and cross-linking agent is used to form a polymer network gel in the glass fiber separator, simplifying the formulation and assembly process, and improving the electrode interface contact and Bonding power.
The gel electrolyte battery achieves high cycle performance and capacity retention, reduces the electrode interface impedance, is suitable for applications in irregular surfaces and curved scenarios, and simplifies the battery preparation process, making it suitable for mass production.
Smart Images

Figure CN116093426B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of metal ion batteries, and in particular relates to an electropolymer gel electrolyte battery and a preparation method of the electropolymer gel electrolyte battery. Background Art
[0002] Gel electrolytes possess the cohesiveness of solids and the diffusivity of liquids. With the development of secondary batteries, gel electrolytes not only meet the electrochemical performance requirements of metal-ion batteries and reduce the safety issues caused by organic solvents, but also exhibit flexibility and excellent interfacial contact. Many studies consider them the future direction for high-performance electrolytes and the most likely replacement for organic electrolytes. However, in currently used gel polymer metal secondary battery systems, the two most common in-situ polymerization methods—external UV-initiated photopolymerization and thermally initiated polymerization—are cumbersome and consume large amounts of organic solvents, easily causing environmental pollution during subsequent solvent recovery. Furthermore, batteries assembled with gel electrolytes prepared by these two external transfer methods exhibit poor compatibility at the gel electrolyte / electrode interface, resulting in significant interfacial impedance, which severely affects the overall battery performance.
[0003] While in-situ gel electrolyte preparation strategies are indeed effective, they require relatively harsh reaction conditions, including toxic reagents, high temperatures, or ultraviolet irradiation. Currently, most methods for preparing in-situ polymeric electrolytes for metal secondary batteries involve in-situ polymerization of monomer molecules in a precursor solution on the electrode surface, followed by gelation and assembly into a battery, thereby obtaining a gel polymer electrolyte capable of conducting metal ions. This in-situ polymerization method enhances the interfacial electrical contact performance between the electrolyte and electrode materials, improving the battery's electrochemical performance. However, these methods still require the addition of free radical initiators or oxidizing / reducing agents to the precursor solution. A smaller number of studies involve in-situ polymerization of monomer molecules within the assembled battery, which requires the addition of thermal initiators and heating to promote chemical cross-linking of monomers within the battery. Therefore, neither of these commonly used in-situ polymerization methods effectively simplifies the formulation and battery preparation and assembly process.
[0004] Based on this, a novel method for preparing gel electrolytes is proposed. This method simplifies the formulation of gel precursor solutions and the battery preparation and assembly process, while improving the cycle performance and rate performance of gel electrolyte batteries, which is a technical problem that urgently needs to be solved. Summary of the Invention
[0005] One of the objects of the present invention is to provide a gel electrolyte battery with high cycle performance and capacity retention rate.
[0006] A second object of the present invention is to provide a method for preparing an electropolymerized gel electrolyte battery that can simplify the formulation of the gel precursor solution and the battery preparation and assembly process.
[0007] The technical solution adopted by the present invention to achieve one of the objectives is: to provide an electropolymer gel electrolyte battery, comprising a negative electrode, a positive electrode and a gel electrolyte;
[0008] The negative electrode is a metal electrode; the gel electrolyte is prepared by in-situ polymerization of a gel precursor solution soaked in a diaphragm through electrical signal processing in a battery; the gel precursor solution includes an anionic polymer monomer and a cross-linking agent.
[0009] In response to the problems existing in the prior art, the present invention proposes a technical solution for the purpose of obtaining carbonyl radicals through an electrochemical method and using this electropolymerization process for the in-situ preparation of gel electrolytes in batteries, thereby achieving dual simplification of the gel precursor solution formulation and the battery preparation and assembly process.
[0010] In the electropolymerized gel electrolyte battery provided by the present invention, the gel electrolyte is a quasi-solid structure of a polymer network gel and a glass fiber separator formed by immersing an anionic polymer monomer / crosslinking agent precursor solution into a glass fiber separator and assembling the battery under the processing of multiple electrical signals. Since many monomer molecules contain atoms such as N or O that can provide lone pairs of electrons, or π bonds containing multiple delocalized electrons, during the gel formation process, a charge transfer process occurs between the metal electrode surface and the precursor solution, the gel electrolyte is in full contact with the interface, and the electrode metal ions accept more lone pairs of electrons or multiple delocalized electrons, forming more coordination bonds that bind the two. The electrolyte helps to improve ionic conductivity, reduce the impedance of the electrode interface and the gel electrolyte, and improve the binding force between them. This can also improve the structural stability of the positive and negative electrode materials during the charging and discharging process, making it widely used in various irregular surfaces and curved scenes.
[0011] The technical solution adopted by the present invention to achieve the second purpose is to provide a method for preparing an electropolymer gel electrolyte battery, comprising the following steps:
[0012] S1. preparing a gel precursor solution comprising an anionic polymer monomer and a cross-linking agent;
[0013] S2, impregnating the glass fiber separator with the gel precursor solution to obtain an impregnated separator;
[0014] S3. Assembling the soaked separator, the positive electrode and the metal negative electrode into a battery, and polymerizing the gel precursor solution in situ in the battery to form a gel electrolyte under the treatment of an electrical signal, thereby obtaining an electropolymerized gel electrolyte battery.
[0015] Furthermore, in step S1, the gel precursor solution is prepared according to the following mass percentages: 20-40 wt.% of ion gel monomer, 0.4-1.0 wt.% of cross-linking agent, and the balance is water or organic solvent.
[0016] Furthermore, the anionic polymer monomer is selected from one or more combinations of 2-acrylamide-2-methylpropane sulfonic acid sodium salt, 2-acrylamide-2-methylpropane sulfonic acid zinc salt, acrylic acid sodium salt, methacrylic acid sodium salt, vinyl sulfonic acid sodium salt, styrene sulfonic acid sodium salt and sodium p-vinylbenzene sulfonate.
[0017] In the present invention, an ion gel electrolyte is used, Zn 2+ 、Li + 、Na + and Al 3+ The appropriate cation can be selected based on the electrode's operational requirements; there is no need to add substances containing Cl. - 、ClO4 - 、NO3 - and SO4 2- Metal salts containing anions effectively reduce the generation of byproducts.
[0018] Furthermore, the cross-linking agent is selected from one or more combinations of N,N'-methylenebisacrylamide and its derivatives or ethylene glycol dimethacrylate and its derivatives.
[0019] Furthermore, in step S2, the thickness of the glass fiber separator is 1 to 1.2 mm, and the pore size is 2.5 to 3.0 μm; and the volume of the gel precursor solution accounts for 40 to 50% of the volume of the glass fiber separator.
[0020] In this invention, an ion gel precursor solution is immersed in a glass fiber separator, where it forms a quasi-solid state of polymer network gel and glass fiber separator under electrical signal processing. The polyanion network structure of the gel electrolyte effectively increases the cation transference number, contributing to improved performance of metal ion batteries. It also improves the uniformity of metal ion deposition during charging and effectively inhibits the growth of negative electrode dendrites.
[0021] Preferably, after step S2, the impregnated membrane is placed in a dark, low-temperature environment for 0.5 to 2 hours, and the gel precursor solution is fully impregnated into the glass fiber membrane and the air inside the membrane is expelled by vacuum, pressurization or alternating vacuum-pressurization cycles.
[0022] Furthermore, in step S3, the metal of the metal negative electrode of the battery is selected from one of zinc, lithium, sodium and aluminum.
[0023] Furthermore, in step S3, the positive electrode material of the battery includes a metal oxide or Prussian blue and its derivatives; the metal oxide is selected from one of manganese oxide, titanium oxide, iron oxide, and vanadium oxide.
[0024] Preferably, the preparation process of the positive electrode sheet of the battery is as follows: the evenly ground positive electrode material, acetylene black and polyvinylidene fluoride (PVDF) dissolved in N-methylpyrrolidone are mixed evenly to form a slurry, which is coated on a titanium foil with a thickness of 20 μm, and the coating thickness is 100 to 300 μm. The positive electrode sheet is obtained by drying at 80°C for 12 hours. The mass ratio of the positive electrode material, acetylene black and polyvinylidene fluoride is 8:(1 to 2):(1 to 2).
[0025] Furthermore, in step S3, the battery assembly method is as follows: placing the electrode sheets in a battery shell, placing a soaked glass fiber separator between the positive and negative electrode sheets to separate them, and then packaging the battery to obtain a metal ion battery.
[0026] Preferably, in step S3, the battery is left to stand for 3 to 6 hours after assembly before subsequent operations are performed.
[0027] Furthermore, the electrical signal processing includes: a combination of one or more of constant current charge and discharge processing, cyclic voltammetry processing or electric pulse processing.
[0028] Preferably, the constant current charge and discharge process includes: -2 The current density is 1~5mAh·cm -2 The capacity charge and discharge process takes 6 to 20 hours;
[0029] Preferably, the cyclic voltammetry treatment comprises: cycling 8 to 30 times in the range of -1 to 1 V at a scan rate of 1 to 10 mV / s;
[0030] Preferably, the electric pulse treatment includes: firstly -2 The current density is constant current charging, the time interval is 0.05~0.5s, stand for 1~2s, and then charge at 8~40mA·cm -2 The current density is constant current discharge, the time interval is 0.05 to 0.5s, and the above operation is repeated. The treatment time is 4 to 5 hours.
[0031] In the present invention, the electrical signal processing method and specific parameters can be configured based on the type of anode metal and the volume of the precursor solution. Generally, for more active metal anodes, cyclic voltammetry and electric pulse treatments achieve better results. Increasing / decreasing the precursor solution volume requires appropriately increasing / decreasing the processing time.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] (1) The electropolymerized gel electrolyte battery and its preparation method provided by the present invention generate carbonyl radicals from gel monomers by electrochemical methods. No free radical initiator is required. Only an appropriate amount of cross-linking agent needs to be added. This electropolymerization process can be used for the in-situ preparation of gel electrolytes, thereby simplifying the formula of the gel precursor solution.
[0034] (2) The electropolymerized gel electrolyte battery and its preparation method provided by the present invention contain N or O atoms that can provide lone pairs of electrons, or π bonds containing multiple delocalized electrons in the monomer molecules in the gel precursor. During the formation of the electropolymerized gel electrolyte, the electrode surface and the precursor solution undergo a charge transfer process, and the gel electrolyte and the interface are in full contact. The electrode metal ions accept more lone pairs of electrons or multiple delocalized electrons, forming more coordination bonds that bind the two together. This helps to improve the ionic conductivity, reduce the impedance of the electrode interface and the gel electrolyte, and improve the bonding force between them. This also improves the structural stability of the positive and negative electrode materials during the charging and discharging process, making it widely applicable to various irregular surfaces and bending scenarios.
[0035] (3) In the preparation method of the electropolymerized gel electrolyte battery provided by the present invention, the gel stock solution immersed in the glass fiber membrane can form a polymer network gel under the processing of various electrical signals, and the polymerization mode is diverse and flexible. After assembling the battery with the glass fiber membrane immersed in the gel precursor solution, a composite quasi-solid structure membrane is formed by electrotreatment, which makes the preparation and assembly process of the gel electrolyte battery simpler and more efficient, and suitable for large-scale production applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is the cycle curve of the zinc symmetrical battery prepared in Example 1 of the present invention;
[0037] Figure 2 The cycling curve of the zinc symmetric battery obtained in Example 2 of this invention;
[0038] Figure 3 This is the cycle curve of the zinc symmetrical battery prepared in Example 3 of the present invention;
[0039] Figure 4 This is a cycle performance diagram of the zinc full battery prepared in Example 4 of the present invention;
[0040] Figure 5 This is a cycle performance diagram of the zinc full battery prepared in Example 5 of the present invention;
[0041] Figure 6 This is the cycle curve of the zinc symmetrical battery prepared in Comparative Example 1 of the present invention;
[0042] Figure 7This is the cycle curve of the zinc symmetrical battery prepared in Comparative Example 2 of the present invention;
[0043] Figure 8 The circuit performance diagram shows the zinc full battery prepared in Comparative Example 1 of this invention.
[0044] Figure 9 The diagram shows the cycle performance of the zinc full battery prepared in Comparative Example 2 of this invention.
[0045] Figure 10 The coin cells prepared in Example 1, Comparative Example 1, and Comparative Example 2 of this invention are compared at different cycles (1 mA·cm). -2 1mAh·cm -2 Comparison of impedance changes after constant current charge and discharge; (a) is the electropolymerized gel electrolyte battery of Example 1; (b) is the UV-polymerized gel electrolyte battery of Comparative Example 1; (c) is the gel monomer solution battery of Comparative Example 2;
[0046] Figure 11 The electropolymerized gel electrolyte prepared by the electrochemical polymerization method provided in this invention and the ultraviolet photopolymerized gel electrolyte were prepared at 1 mA·cm -2 1mAh·cm -2 Comparison of the test results of zinc sheet peeling force after 60 cycles of constant current charge and discharge. DETAILED DESCRIPTION
[0047] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts shall fall within the scope of protection of the present invention.
[0048] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features therein may be combined with each other.
[0049] The present invention will be further described below with reference to specific embodiments. The embodiments take zinc ion batteries as an example, but are not intended to limit the present invention. Metal ion batteries such as lithium, sodium, and aluminum are also applicable.
[0050] The battery types, polymerization methods, and electrical treatment methods of Examples 1-5 and Comparative Examples 1 and 2 are shown in Table 1 below.
[0051] Table 1
[0052]
[0053]
[0054] Example 1
[0055] Step 1: Prepare a hydrogel precursor aqueous solution containing ion gel monomers and cross-linking agents:
[0056] 20.7 g of 2-acrylamido-2-methylpropanesulfonic acid and 0.4 g of N,N'-methylenebisacrylamide were dissolved in 50 mL of deionized water and stirred at 60 °C for 30 min. Then, 5 g of zinc oxide was slowly added to the solution and stirred for 30 min. The excess zinc oxide was separated by centrifugation (6000 r / min) to obtain an aqueous solution of an electropolymerization ionogel precursor containing zinc 2-acrylamido-2-methylpropanesulfonic acid salt.
[0057] Step 2: Infiltrate the glass fiber separator with the gel precursor solution and assemble the symmetrical battery:
[0058] A glass fiber diaphragm with a thickness of 1±0.5 mm and a pore size of 2.7 μm was selected and cut into discs with a diameter of 1.6 cm. 45 μL of ion gel precursor aqueous solution was added to each side. The wetted diaphragm was placed in a light-proof, low-temperature environment for 1 hour and then transferred to a vacuum box. The vacuum was evacuated to 0.01 MPa and the pressure was maintained for 20 minutes. Nitrogen was passed through the box and loaded into a CR2032 button battery with zinc sheets (thickness 0.1 mm) for both the negative and positive electrodes to assemble into a symmetrical battery.
[0059] Step 3: Preparation of electropolymerized gel electrolyte battery by electrical treatment:
[0060] After the zinc symmetric battery was assembled, it was left to stand for 5 hours and the current was set to 1 mA·cm -2 1mAh·cm -2 The constant current charge and discharge treatment conditions were set at 8 hours to obtain an electropolymer gel electrolyte battery.
[0061] Example 2
[0062] Step 1: Prepare a hydrogel precursor aqueous solution containing ion gel monomers and cross-linking agents:
[0063] 20.7 g of 2-acrylamido-2-methylpropanesulfonic acid and 0.4 g of N,N'-methylenebisacrylamide were dissolved in 50 mL of deionized water and stirred at 60 °C for 30 min. Then, 5 g of zinc oxide was slowly added to the solution and stirred for 30 min. The excess zinc oxide was separated by centrifugation (6000 r / min) to obtain an aqueous solution of an electropolymerization ionogel precursor containing zinc 2-acrylamido-2-methylpropanesulfonic acid salt.
[0064] Step 2: Infiltrate the glass fiber separator with the gel precursor solution and assemble the symmetrical battery:
[0065] A glass fiber diaphragm with a thickness of 1±0.5 mm and a pore size of 2.7 μm was selected and cut into discs with a diameter of 1.6 cm. 45 μL of ion gel precursor aqueous solution was added to each side. The wetted diaphragm was placed in a light-proof, low-temperature environment for 1 hour and then transferred to a vacuum box. The vacuum was evacuated to 0.01 MPa and the pressure was maintained for 20 minutes. Nitrogen was passed through the box and loaded into a CR2032 button battery with zinc sheets (thickness 0.1 mm) for both the negative and positive electrodes to assemble into a symmetrical battery.
[0066] Step 3: Preparation of electropolymerized gel electrolyte battery by electrical treatment:
[0067] After the zinc symmetric battery was assembled, it was allowed to stand for 5 hours, and the cyclic voltammetry treatment conditions were set at a scan rate of 1 mV / s and within a range of -1 to 1 V. The cycle was repeated 18 times to obtain an electropolymerized gel electrolyte battery.
[0068] Example 3
[0069] Step 1: Prepare a hydrogel precursor aqueous solution containing ion gel monomers and cross-linking agents:
[0070] 20.7 g of 2-acrylamido-2-methylpropanesulfonic acid and 0.4 g of N,N'-methylenebisacrylamide were dissolved in 50 mL of deionized water and stirred at 60 °C for 30 min. Then, 5 g of zinc oxide was slowly added to the solution and stirred for 30 min. The excess zinc oxide was separated by centrifugation (6000 r / min) to obtain an aqueous solution of an electropolymerization ionogel precursor containing zinc 2-acrylamido-2-methylpropanesulfonic acid salt.
[0071] Step 2: Infiltrate the glass fiber separator with the gel precursor solution and assemble the symmetrical battery:
[0072] A glass fiber diaphragm with a thickness of 1±0.5 mm and a pore size of 2.7 μm was selected and cut into discs with a diameter of 1.6 cm. 45 μL of ion gel precursor aqueous solution was added to each side. The wetted diaphragm was placed in a light-proof, low-temperature environment for 1 hour and then transferred to a vacuum box. The vacuum was evacuated to 0.01 MPa and the pressure was maintained for 20 minutes. Nitrogen was passed through the box and loaded into a CR2032 button battery with zinc sheets (thickness 0.1 mm) for both the negative and positive electrodes to assemble into a symmetrical battery.
[0073] Step 3: Preparation of electropolymerized gel electrolyte battery by electrical treatment:
[0074] After the zinc symmetrical battery was assembled, it was left to stand for 5 hours and the current was set to 10 mA cm -2 Constant current charging, time interval 0.1s, standstill 1s, 10mA·cm -2 The electropolymerized gel electrolyte battery was obtained by constant current discharge, electric pulse treatment with a time interval of 0.1s, and treatment time of 5 hours.
[0075] Example 4
[0076] Step 1: Prepare a hydrogel precursor aqueous solution containing ion gel monomers and cross-linking agents:
[0077] 20.7 g of 2-acrylamido-2-methylpropanesulfonic acid and 0.4 g of N,N'-methylenebisacrylamide were dissolved in 50 mL of deionized water and stirred at 60 °C for 30 min. Then, 5 g of zinc oxide was slowly added to the solution and stirred for 30 min. The excess zinc oxide was separated by centrifugation (6000 r / min) to obtain an aqueous solution of an electropolymerization ionogel precursor containing zinc 2-acrylamido-2-methylpropanesulfonic acid salt.
[0078] Step 2: Infiltrate the glass fiber separator with the gel precursor solution and assemble the full battery:
[0079] A glass fiber diaphragm with a thickness of 1±0.5 mm and a pore size of 2.7 μm was selected and cut into discs with a diameter of 1.6 cm. 45 μL of ion gel precursor aqueous solution was added to each side. The wetted diaphragm was placed in a light-proof, low-temperature environment for 1 hour and then transferred to a vacuum box. The vacuum was evacuated to 0.01 MPa and the pressure was maintained for 20 minutes. Nitrogen was passed through the box and loaded into a CR2032 button battery with a zinc sheet (thickness of 0.1 mm) as the negative electrode and a titanium foil (thickness of 20 μm) with a positive electrode coating adhered to the positive electrode to form a full battery.
[0080] The prepared positive electrode coating film on titanium foil had a wet film thickness of 50±5 μm. After drying at 80℃ for 12 hours, it was cut into circular pieces with a diameter of 12 mm to obtain the positive electrode sheet. The composition of the positive electrode coating film included 80 wt.% manganese dioxide active material, 10 wt.% acetylene black conductive agent, and 10 wt.% polyvinylidene fluoride binder. The loading of active material on the positive electrode sheet was 0.64–0.72 mg.
[0081] Step 3: Preparation of electropolymerized gel electrolyte battery by electrical treatment:
[0082] After the zinc full battery was assembled, it was allowed to stand for 5 hours, and the cyclic voltammetry treatment conditions were set at a scan rate of 1 mV / s and a range of 0 to 2 V. The cycle was repeated 18 times to obtain an electropolymerized gel electrolyte battery.
[0083] Example 5
[0084] Step 1: Prepare a hydrogel precursor aqueous solution containing ion gel monomers and cross-linking agents:
[0085] 20.7 g of 2-acrylamido-2-methylpropanesulfonic acid and 0.4 g of N,N'-methylenebisacrylamide were dissolved in 50 mL of deionized water and stirred at 60 °C for 30 min. Then, 5 g of zinc oxide was slowly added to the solution and stirred for 30 min. The excess zinc oxide was separated by centrifugation (6000 r / min) to obtain an aqueous solution of an electropolymerization ionogel precursor containing zinc 2-acrylamido-2-methylpropanesulfonic acid salt.
[0086] Step 2: Infiltrate the glass fiber separator with the gel precursor solution and assemble the full battery:
[0087] A glass fiber diaphragm with a thickness of 1±0.5 mm and a pore size of 2.7 μm was selected and cut into discs with a diameter of 1.6 cm. 45 μL of ion gel precursor aqueous solution was added to each side. The wetted diaphragm was placed in a light-proof, low-temperature environment for 1 hour and then transferred to a vacuum box. The vacuum was evacuated to 0.01 MPa and the pressure was maintained for 20 minutes. Nitrogen was passed through the box and loaded into a CR2032 button battery with a zinc sheet (thickness of 0.1 mm) as the negative electrode and a titanium foil (thickness of 20 μm) with a positive electrode coating adhered to the positive electrode to form a full battery.
[0088] The prepared positive electrode coating film on titanium foil had a wet film thickness of 50±5 μm. After drying at 80℃ for 12 hours, it was cut into circular pieces with a diameter of 12 mm to obtain the positive electrode sheet. The composition of the positive electrode coating film included 80 wt.% manganese dioxide active material, 10 wt.% acetylene black conductive agent, and 10 wt.% polyvinylidene fluoride binder. The loading of active material on the positive electrode sheet was 0.64–0.72 mg.
[0089] Step 3: Preparation of electropolymerized gel electrolyte battery by electrical treatment:
[0090] After the zinc full cell is assembled, it is left to stand for 5 hours and then set to 1 mA·cm. -2 Constant current discharge to 1.8V, 1mA·cm -2 A constant current charge-discharge process was performed under constant current charging conditions down to 0.2V, and the cycle was repeated 12 times to obtain an electropolymerized gel electrolyte battery.
[0091] Comparative Example 1
[0092] Step 1: Preparation of aqueous solution of UV-polymerized gel electrolyte precursor:
[0093] 20.7 g of 2-acrylamido-2-methylpropanesulfonic acid, 0.4 g of N,N'-methylenebisacrylamide, and 0.4 g of 2-hydroxy-2-methyl-1-phenyl ketone were dissolved in 50 mL of deionized water and stirred at 60 °C for 30 min. Then, 5 g of zinc oxide was slowly added to the solution and stirred for 30 min. The excess zinc oxide was separated by centrifugation (6000 r / min) to obtain an aqueous solution of the UV-polymerized ionogel precursor containing zinc 2-acrylamido-2-methylpropanesulfonic acid salt.
[0094] Step 2: UV-polymerized ion gel precursor aqueous solution is photopolymerized in a glass fiber separator and then assembled into symmetric cells and full cells:
[0095] A glass fiber membrane with a thickness of 1±0.5 mm and a pore size of 2.7 μm was selected and cut into circular pieces with a diameter of 1.6 cm. 45 μL of UV-photopolymerized ionogel precursor aqueous solution was dropped onto each side. The wetted membrane was placed in a light-proof, low-temperature environment for 1 hour and then transferred to a vacuum chamber. The vacuum was evacuated to 0.01 MPa and held for 20 min. Nitrogen gas was then introduced, and the wetted membrane was transferred to a glass container. Nitrogen gas was introduced, and the container was sealed after the glass container was filled with a nitrogen atmosphere. The container was then placed under a 365 nm UV lamp for 8 hours to obtain a photopolymerized hydrogel electrolyte membrane of composite glass fiber paper. This membrane was then installed in a CR2032 button cell with zinc sheets (0.1 mm thick) as both the positive and negative electrodes to assemble a symmetrical cell.
[0096] In addition, a full cell is assembled by inserting a CR2032 button cell into a zinc sheet (0.1 mm thick) as the negative electrode and a titanium foil (20 μm thick) with a positive electrode coating adhered to it.
[0097] The prepared positive electrode coating film on titanium foil had a wet film thickness of 50±5 μm. After drying at 80℃ for 12 hours, it was cut into circular pieces with a diameter of 12 mm to obtain the positive electrode sheet. The composition of the positive electrode coating film included 80 wt.% manganese dioxide active material, 10 wt.% acetylene black conductive agent, and 10 wt.% polyvinylidene fluoride binder. The loading of active material on the positive electrode sheet was 0.64–0.72 mg.
[0098] Comparative Example 2
[0099] Step 1: Preparation of monomeric solution electrolyte:
[0100] 20.7 g of 2-acrylamido-2-methylpropanesulfonic acid was dissolved in 50 mL of deionized water and stirred at 60 °C for 30 min. Then, 5 g of zinc oxide was slowly added to the solution and stirred for 30 min. The excess zinc oxide was separated by centrifugation (6000 r / min) to obtain a solution electrolyte with zinc salt of 2-acrylamido-2-methylpropanesulfonic acid as the monomer.
[0101] Step 2: After immersing the monomer solution electrolyte into the glass fiber membrane, assemble the symmetrical cell and the full cell:
[0102] A glass fiber diaphragm with a thickness of 1±0.5 mm and a pore size of 2.7 μm was selected and cut into discs with a diameter of 1.6 cm. 45 μL of monomer solution was added to each side of the membrane. The wetted membrane was placed in a dark, low-temperature environment for 1 hour and then transferred to a vacuum box. The membrane was evacuated to 0.01 MPa and the pressure was maintained for 20 minutes. Nitrogen was passed through the box and placed in a CR2032 button battery with zinc sheets (thickness 0.1 mm) for both the negative and positive electrodes to form a symmetrical battery.
[0103] In addition, a full cell is assembled by inserting a CR2032 button cell into a zinc sheet (0.1 mm thick) as the negative electrode and a titanium foil (20 μm thick) with a positive electrode coating adhered to it.
[0104] The prepared positive electrode coating film on titanium foil had a wet film thickness of 50±5 μm. After drying at 80℃ for 12 hours, it was cut into circular pieces with a diameter of 12 mm to obtain the positive electrode sheet. The composition of the positive electrode coating film included 80 wt.% manganese dioxide active material, 10 wt.% acetylene black conductive agent, and 10 wt.% polyvinylidene fluoride binder. The loading of active material on the positive electrode sheet was 0.64–0.72 mg.
[0105] Performance Testing
[0106] (1) Cycle and capacity performance test
[0107] The zinc symmetric cells prepared in Examples 1-3 were subjected to 1 mA·cm -2 The constant current cycle charge-discharge test was conducted at a current density of 1 mAh·cm³. -2 The batteries prepared in Examples 4 and 5 were subjected to constant current charge-discharge tests, with a constant current density of 0.1 A·g. -1 .
[0108] The zinc symmetric cells prepared in Examples 1 and 2 were subjected to a 1 mA·cm test. -2 Constant current cycle charge-discharge test at current density (charge-discharge capacity set at 1 mAh·cm³) -2 The zinc full cells prepared in Examples 1 and 2 were subjected to constant current charge-discharge tests (the constant current density was set to 0.1 A·g). -1 ).
[0109] The test results are as follows Figure 1-10 shown.
[0110] Depend on Figure 1-3 、 Figure 6 and Figure 7By comparing the test results of the symmetrical batteries of Examples 1-3 with those of Comparative Examples 1 and 2, it can be seen that the symmetrical batteries of Examples 1-3 all have a cycle life of more than 2000 hours, while the symmetrical batteries of Comparative Examples 1 and 2 are mainly interrupted by short circuits caused by dendrite growth, which indicates that the electropolymerized gel electrolyte provided by the present invention can make the zinc ion dissolution / deposition process occur uniformly, which can effectively solve the problem of zinc dendrite growth.
[0111] Depend on Figure 4 、 Figure 5 、 Figure 8 and Figure 9 By comparing the full batteries of Examples 4 and 5 with the full batteries of Comparative Examples 1 and 2, it can be seen that the electropolymerized gel electrolyte enables the aqueous zinc ion full battery to have relatively better cycle performance, and has a significantly higher capacity retention rate than the full battery of UV-polymerized gel electrolyte and the monomer solution electrolyte that cannot be gelled. This shows that the electropolymerized gel electrolyte also plays a certain degree of protective role on the positive electrode of the metal ion battery.
[0112] Further, Figure 10 (a)(b)(c) represent the symmetrical cells of Example 1, Comparative Example 1, and Comparative Example 2, respectively, at 1 mA·cm⁻¹. -2 1mAh·cm -2 Impedance tests were conducted immediately after constant current charge and discharge cycles (2, 5, 10, 30, and 60 cycles). The impedance changes after constant current charge and discharge for the three groups of samples showed that the electropolymerized gel electrolyte battery had a smaller capacitive arc radius after each cycle, indicating a lower charge transfer resistance at the interface, especially after 5 cycles. This shows that the electropolymerized gel electrolyte of the present invention improves zinc negative electrode problems such as corrosion and passivation, allowing the electrode surface to maintain a better activation state for a long time, thereby stabilizing the zinc negative electrode surface.
[0113] (2) Peeling test
[0114] The glass fiber diaphragm was cut to a length of 70 mm and a width of 40 mm. 630 μL of an aqueous solution of the electropolymerized ionogel precursor was dropped onto each side. Two zinc sheets, 40–60 mm long and 20–30 mm wide and polished to 2000 mesh, were sandwiched between the two sides of the diaphragm to form a three-layer structure of zinc sheet / glass fiber diaphragm / zinc sheet. This three-layer structure was then clamped together with two 100×100 mm glass plates, leaving a 10 mm long side for connecting to an external power source. A 1 mA·cm² power supply was set. -2 1mAh·cm -2The constant current charge and discharge treatment conditions were followed, and the glass plates were removed after 120 hours (60 cycles). The remaining parts of the two zinc sheets were fixed on the two fixtures of the peeling force tester, and then the peeling test was performed at a speed of 1mm / min and a load of 10N until the three-layer structure was peeled off. In addition, 630μL of an aqueous solution of ultraviolet-polymerized ion gel precursor was dripped onto the front and back sides of a glass fiber diaphragm of the same size, and the wetted diaphragm was photopolymerized using the method described in Comparative Example 1. Similarly, two zinc sheets with a length of 40-60mm and a width of 20-30mm were polished to 2000 mesh and clamped in the middle of both sides of the diaphragm to form a three-layer structure of zinc sheet / glass fiber diaphragm / zinc sheet. The three-layer structure was clamped with two 100×100mm glass plates, and subjected to the same constant current charge and discharge treatment and peeling test. The test results are as follows Figure 11 shown.
[0115] Depend on Figure 11 It can be seen that the peeling experiment shows that after the same electrical treatment (1mA·cm -2 1mAh·cm -2 (Constant current charge-discharge for 60 cycles) The electropolymerized gel electrolyte prepared by the electrochemical polymerization method provided in this invention has a stronger adhesion to the zinc electrode than the ultraviolet light polymerized electrolyte. Its adhesion to the zinc electrode is about twice that of the ultraviolet light polymerized electrolyte. This indicates that the electropolymerized gel electrolyte battery is more suitable for various irregular surfaces and bending scenarios.
[0116] In summary, the gel electrolyte battery provided by the present invention has excellent cycle performance and capacity retention, stabilizes the zinc negative electrode surface, and has stronger adhesion between the gel electrolyte and the electrode sheet, with strong peeling resistance, making it more suitable for application on various irregular surfaces and curved environments. Importantly, the preparation method uses simplified and readily available raw material components, and the battery assembly steps are simple, making it suitable for large-scale production and promising broad prospects for promotion and application.
[0117] The above are merely preferred embodiments of the present invention and are not intended to limit the implementation methods and protection scope of the present invention. Those skilled in the art should recognize that any equivalent substitutions and obvious changes made based on the content of this specification should be included within the protection scope of the present invention.
Claims
1. An electropolymer gel electrolyte battery, comprising a negative electrode, a positive electrode and a gel electrolyte; characterized in that: The negative electrode is a metal electrode; the metal of the metal electrode is selected from one of zinc, lithium, sodium and aluminum; The gel electrolyte is prepared by in-situ polymerization of a gel precursor solution soaked in a separator in a battery through electrical signal processing; The gel precursor solution is prepared according to the following mass percentages: 20-40 wt.% of anionic polymer monomer, 0.4-1.0 wt.% of cross-linking agent, and the balance is water or organic solvent; The anionic polymer monomer is selected from one or more combinations of 2-acrylamide-2-methylpropane sulfonic acid sodium salt, 2-acrylamide-2-methylpropane sulfonic acid zinc salt, ethylene sulfonic acid sodium salt, styrene sulfonic acid sodium salt and sodium p-vinylbenzene sulfonate.
2. A method for preparing an electropolymer gel electrolyte battery, comprising the following steps: S1, preparing a gel precursor solution containing anionic polymer monomers and a cross-linking agent; S2, infiltrating the gel precursor solution into a glass fiber separator to obtain an infiltrated separator; S3, assembling the impregnated separator, the positive electrode and the metal negative electrode into a battery, and polymerizing the gel precursor solution in situ in the battery to form a gel electrolyte under the treatment of an electrical signal, thereby obtaining an electropolymerized gel electrolyte battery; The metal of the metal negative electrode is selected from one of zinc, lithium, sodium and aluminum; The gel precursor solution is prepared according to the following mass percentages: 20-40 wt.% of anionic polymer monomer, 0.4-1.0 wt.% of cross-linking agent, and the balance is water or organic solvent; The anionic polymer monomer is selected from one or more combinations of 2-acrylamide-2-methylpropane sulfonic acid sodium salt, 2-acrylamide-2-methylpropane sulfonic acid zinc salt, ethylene sulfonic acid sodium salt, styrene sulfonic acid sodium salt and sodium p-vinylbenzene sulfonate.
3. The preparation method according to claim 2, characterized in that: The crosslinking agent is selected from one or more combinations of N,N'-methylenebisacrylamide and its derivatives or ethylene glycol dimethacrylate and its derivatives.
4. The preparation method according to claim 2, characterized in that: In step S2, the thickness of the glass fiber diaphragm is 1-1.2 mm, and the pore size is 2.5-3.0 μm; the volume of the gel precursor solution accounts for 40-50% of the volume of the glass fiber diaphragm.
5. The preparation method according to claim 2, characterized in that: The electrical signal processing includes: a constant current charge and discharge process, a cyclic voltammetry process or an electrical pulse process or a combination of one or more of the above.
6. The preparation method according to claim 5, characterized in that The constant current charge and discharge process includes: -2 The current density is 1~5 mAh·cm -2 The capacity is charged and discharged, and the processing time is 6 to 20 hours.
7. The preparation method according to claim 5, characterized in that The cyclic voltammetry treatment includes: cycling 8 to 30 times in the range of -1 to 1 V at a scan rate of 1 to 10 mV / s.
8. The preparation method according to claim 5, characterized in that The electric pulse treatment includes: firstly, 8-40 mA·cm -2 The current density was 8~40 mA·cm -2 The current density is discharged at a constant current, with a time interval of 0.05~0.5 s. The above operation is repeated for a treatment time of 4~5 hours.
Citation Information
Cited By
Composition, gel electrolyte for solid-state battery, gel electrolyte for solid-state battery, preparation method of gel electrolyte, solid-state battery, preparation method of solid-state battery and electric device
CN122696775A