Epoxy stick adhesive with rapid debonding at room temperature and preparation method thereof
By introducing silane coupling agent-modified sodium bicarbonate and heavy calcium carbonate composite particles into the adhesive rod as a debinding agent, and utilizing its reaction with lactic acid to form a salt effect, rapid debinding at room temperature is achieved, solving the problems of high energy consumption and silicon wafer oxidation in high-temperature debinding, and meeting the requirements of silicon wafer cutting process.
Patent Information
- Application Number
- CN202211678688.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-26
AI Technical Summary
Existing adhesive rods consume a lot of energy when debonding under high temperature conditions and are prone to oxidation of the silicon wafer surface, which affects the photoelectric conversion efficiency of photovoltaic cells and increases manufacturing costs.
The epoxy adhesive rod uses components A and B. Component B uses sodium bicarbonate and heavy calcium carbonate composite microparticles with silane coupling agent surface modification as degumming agents. It achieves rapid degumming by reacting with lactic acid at room temperature to form a salt effect.
It enables rapid debinding at room temperature, avoids oxidation of the silicon wafer surface, simplifies operation, saves costs, and meets the requirements of silicon wafer cutting processes.
Smart Images

Figure GDA0004161631940000061 
Figure GDA0004161631940000071 
Figure GDA0004161631940000081
Abstract
Description
Technical Field
[0001] The invention relates to the field of adhesives, and in particular to an epoxy stick adhesive capable of rapid debonding at room temperature and a preparation method thereof. Background Art
[0002] Against the backdrop of global warming and the depletion of fossil energy, photovoltaic power generation has the advantages of sustainable resources, environmental friendliness, and no geographical restrictions. The annual newly installed capacity accounts for more than half of the new energy. Silicon wafers are important components of photovoltaic solar cells. The raw materials and production costs account for about 50% of the entire photovoltaic module. Its quality directly affects the photovoltaic conversion efficiency of the battery. Silicon wafer cutting includes processes such as silicon rod bonding and fixing-diamond multi-wire cutting-water washing and degumming. As an indispensable auxiliary material in the silicon wafer cutting process, stick glue greatly affects the efficiency, yield, yield and cost of silicon wafer production. Therefore, requirements such as strong bonding, good water resistance, high hardness and fast degumming are put forward for stick glue.
[0003] In recent years, a lot of research has been carried out on how to improve the degumming speed of stick glue, but all of them achieve the separation of silicon wafer and colloid by softening the colloid at high temperature. Commercially available stick glue products generally need to be degummed by acid boiling at above 50°C. Patent CN109321185A adds sodium polyacrylate and polyacrylamide as degumming factors, and degummes by high-temperature water boiling at 60-80°C. The high degumming temperature not only consumes a lot of energy, but more importantly, it is easy to oxidize the surface of the silicon wafer, which directly affects the quality and yield of the silicon wafer, reduces the photoelectric conversion efficiency of solar cells and increases manufacturing costs. Summary of the invention
[0004] The present invention aims to provide an epoxy adhesive stick adhesive with rapid degumming at room temperature and a preparation method thereof, so as to realize rapid acid boiling degumming at room temperature.
[0005] To achieve the above-mentioned purpose, the present invention adopts the following technical scheme: an epoxy stick adhesive with rapid degumming at room temperature, comprising component A and component B, wherein component A comprises the following raw materials in parts by mass: 30-70 parts of epoxy resin, 30-60 parts of filler, 0.01-2 parts of anti-settling agent, and 0.01-1 parts of defoaming agent; component B comprises the following raw materials in parts by mass: 20-70 parts of polythiol, 10-20 parts of degumming factor, 1-10 parts of accelerator, 0.05-2 parts of coupling agent, 20-60 parts of filler, 0.01-2 parts of anti-settling agent, and 0.01-1 parts of defoaming agent; the degumming factor is sodium bicarbonate and heavy calcium composite particles surface-modified by a silane coupling agent.
[0006] On the other hand, the technical solution also provides a method for preparing epoxy adhesive stick adhesive with rapid debonding at room temperature, comprising the following steps:
[0007] Step 1: Preparation of component A: proportioning and mixing the materials of component A;
[0008] Step 2, preparation of component B: using a silane coupling agent to modify the surface of sodium bicarbonate and heavy calcium to obtain degumming factor composite particles, and then proportioning and mixing the materials of component B;
[0009] Step 3: Mixing component A and component B.
[0010] Preferably, as an improvement, the mass ratio of component A to component B is 1:0.5-2.
[0011] Preferably, as an improvement, the preparation method of the degumming factor comprises the following steps:
[0012] S1, mixing heavy calcium and sodium bicarbonate and grinding;
[0013] S2. Add silane coupling agent for surface modification in multiple times, and the mass ratio of the total amount of silane coupling agent added to sodium bicarbonate is 1-5:100.
[0014] Preferably, as an improvement, in step S1, the mass ratio of heavy calcium to sodium bicarbonate is 1:1-5.
[0015] In this technical solution, the mass ratio of heavy calcium carbonate to sodium bicarbonate is limited mainly for practical effect and grinding effect considerations. Too much calcium carbonate will affect the degumming rate; too little sodium bicarbonate will cause hardening and decomposition during grinding.
[0016] Preferably, as an improvement, in step S1, the grinding conditions are temperature ≤ 50°C and humidity ≤ 25%.
[0017] In this technical solution, too high a temperature during the grinding process will cause sodium bicarbonate to decompose, and too high a humidity will cause hardening, which will affect the particle size of the particles after grinding.
[0018] Preferably, as an improvement, in step S2, the surface is modified and then sieved to obtain composite particles of sodium bicarbonate and calcium carbonate modified by a silane coupling agent with a particle size of less than 20 μm.
[0019] Preferably, as an improvement, the epoxy resin is at least one of E-20, E-44, E-51, E-54, and E-56; the filler is at least one of calcium carbonate, silicon powder, talc, alumina, aluminum hydroxide, and silicon dioxide; the defoamer is at least one of fumed silica, organic bentonite, and hydrogenated castor oil; and the defoamer is at least one of 853, 554, and L-632.
[0020] Preferably, as an improvement, the polythiol is at least one of R2000, R2020, and 830; the promoter is at least one of triethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, pyridine, resorcinol, m-cresol, and phenol; and the coupling agent is at least one of KH550 and KH592.
[0021] Preferably, as an improvement, the mixing process of step 1 and step 2 is performed under vacuum conditions.
[0022] The principle and advantages of this solution are: high-temperature water boiling and high-temperature acid boiling are important ways to achieve rapid debonding of currently available adhesive stick products. From the perspective of energy, high temperature means that the debonding liquid needs to be heated, which consumes a lot of energy. From the perspective of cost, the heating link requires a one-time investment in equipment and continuous consumption of electricity. Based on both energy and cost factors, a kind of adhesive stick that can achieve rapid debonding at room temperature and reduce production costs is developed. In the process of technical research and development, how to achieve rapid debonding at room temperature is the difficulty of this technical solution. The use of heating to soften the colloid and weaken the interfacial adhesion in the existing debonding technology does not meet the purpose of room temperature debonding, so it is necessary to find a new driving force for debonding. In the process of technical development, it was found that most of the factors that are beneficial to debonding will reduce the water resistance of the material, making the comprehensive performance of the colloid not meet the requirements of the cutting process. Benefiting from the inspiration of the relevant literature on foaming agents, the foaming material sodium bicarbonate is introduced into the system, and its reaction with lactic acid in the debonding liquid is cleverly used to replace the conditions of high-temperature decomposition. Not only that, sodium bicarbonate can form a salt effect with lactic acid to accelerate the reaction. In actual applications, it is found that the particles are too large and unevenly distributed, so mixed grinding and surface modification were carried out to solve related application problems.
[0023] The beneficial effects of this technical solution are:
[0024] 1. This technical solution innovatively introduces modified sodium bicarbonate and heavy calcium composite particles as degumming factors, which can form a salt effect with lactic acid in the degumming solution currently used in industrial applications, accelerate the generation of gas, form a strong degumming driving force, and achieve rapid acid boiling degumming at room temperature (≥20°C), effectively avoiding oxidation of the silicon wafer surface under high temperature conditions, affecting the yield rate of the silicon wafer cutting process. At the same time, the system can achieve rapid degumming above 20°C, and the heating process can be omitted during the degumming process, simplifying the operation and saving costs.
[0025] 2. This technical solution adopts sodium bicarbonate and heavy calcium mixed and ground in an appropriate proportion, controls the reaction temperature and humidity, and effectively solves the problems of agglomeration and decomposition in the grinding process of sodium bicarbonate. Silane coupling agent is added in batches to modify the composite particles of sodium bicarbonate and heavy calcium, which plays a role in grinding and forms an organic-coated surface, reduces the loss of the ball mill and effectively solves the dispersion and storage stability problems of the particles in the system. DETAILED DESCRIPTION
[0026] The following is further described in detail through specific implementations, but the implementation of the present invention is not limited thereto. Unless otherwise specified, the technical means used in the following implementations are conventional means well known to those skilled in the art; the experimental methods used are all conventional methods; the materials, reagents, etc. used can all be obtained from commercial channels.
[0027] Program Overview:
[0028] A room temperature fast degumming epoxy stick adhesive comprises component A and component B. Component A comprises the following raw materials in parts by mass: 30-70 parts of epoxy resin, 30-60 parts of filler, 0.01-2 parts of anti-settling agent, and 0.01-1 parts of defoamer; component B comprises the following raw materials in parts by mass: 20-70 parts of polythiol, 10-20 parts of degumming factor, 1-10 parts of accelerator, 0.05-2 parts of coupling agent, 20-60 parts of filler, 0.01-2 parts of anti-settling agent, and 0.01-1 parts of defoamer. The degumming factor in component B is sodium bicarbonate and heavy calcium composite particles surface-modified by silane coupling agent.
[0029] The heavy calcium and sodium bicarbonate in the degumming factor are both commercially available products, and the silane coupling agent is a commercially available silane coupling agent containing an amino group or a mercapto group. The preparation process of the degumming factor includes the following steps:
[0030] S1. Mix heavy calcium and sodium bicarbonate in a mass ratio of 1:1-5 and add them into a ball mill. Grind at a temperature of ≤50°C and a humidity of ≤25%.
[0031] S2. After grinding for a period of time, silane coupling agent is added several times for surface modification. The mass ratio of the total amount of silane coupling agent added to sodium bicarbonate is 1-5:100. Finally, composite particles of sodium bicarbonate and heavy calcium modified by silane coupling agent are obtained, and composite particles with a particle size of less than 20 μm are obtained by sieving.
[0032] The epoxy resin is at least one of E-20, E-44, E-51, E-54, and E-56.
[0033] The filler is at least one of calcium carbonate, silicon powder, talcum powder, aluminum oxide, aluminum hydroxide and silicon dioxide.
[0034] The anti-settling agent is at least one of fumed silica, organic bentonite and hydrogenated castor oil.
[0035] The defoaming agent is at least one of 853, 554, and L-632.
[0036] The polythiol is at least one of R2000, R2020 and 830.
[0037] The accelerator is at least one of triethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, pyridine, resorcinol, m-cresol and phenol.
[0038] The coupling agent is at least one of KH550 and KH592.
[0039] A method for preparing epoxy stick adhesive with rapid debonding at room temperature comprises the following steps:
[0040] Step 1, preparation of component A: the materials of the above-mentioned component A are mixed according to mass ratio, and bisphenol A epoxy resin, filler, anti-settling agent and defoaming agent are added into a planetary agitator, and dispersed and mixed evenly under vacuum conditions to obtain component A.
[0041] Step 2: Preparation of component B:
[0042] The preparation process of the degumming factor comprises the following steps:
[0043] (1) Heavy calcium and sodium bicarbonate are mixed in a mass ratio of 1:1 to 5 and added into a ball mill, and the grinding temperature is controlled to be ≤50°C and the humidity is ≤25% for grinding.
[0044] After grinding for a period of time, silane coupling agent is added several times for surface modification, and the mass ratio of the total amount of silane coupling agent added to sodium bicarbonate is 1-5:100. Finally, composite particles of sodium bicarbonate and heavy calcium modified by silane coupling agent are obtained, and composite particles with a particle size of less than 20 μm are obtained by sieving.
[0045] Then, the materials of the above-mentioned component B are mixed according to mass ratio, and polythiol, degumming factor, accelerator, coupling agent, anti-settling agent, filler and defoaming agent are added into a planetary agitator, and dispersed and mixed evenly under vacuum conditions, and then the component B is obtained.
[0046] Step 3, mixing component A with component B: Component A and component B are uniformly mixed in a weight ratio of A:B=1:0.5-2 to obtain an epoxy-polythiol curing system that can be quickly debonded under mild conditions.
[0047] Example 1
[0048] A room temperature fast debonding epoxy stick adhesive, comprising the following raw materials in parts by weight:
[0049] Component A: 50 parts of bisphenol A epoxy resin, 35 parts of filler, 0.1 parts of anti-settling agent, and 0.1 parts of defoaming agent.
[0050] Component B: 40 parts of polythiol, 20 parts of degumming factor, 2 parts of accelerator, 0.5 parts of coupling agent, 20 parts of filler, 0.2 parts of anti-settling agent, and 0.2 parts of defoaming agent.
[0051] Among them, the bisphenol A type epoxy resin in component A is E-51, the filler is calcium carbonate, the defoamer is 853, and the anti-settling agent is fumed silica. The polythiol in component B is polythiol R-2000, the degumming factor is a composite particle of sodium bicarbonate and heavy calcium modified by a silane coupling agent, the accelerator is DMP-30, the coupling agent is KH550, the filler is calcium carbonate, the defoamer is 853, and the anti-settling agent is fumed silica. The mass ratio of the degumming factor heavy calcium and sodium bicarbonate in component B is 1:1, and the silane coupling agent is 3-aminopropyltriethoxysilane, and the mass ratio with sodium bicarbonate is 1:100.
[0052] A method for preparing epoxy stick adhesive with rapid debonding at room temperature comprises the following steps:
[0053] Step 1, preparation of component A: Add the material composition of component A into a planetary mixer according to the weight ratio, and disperse and mix evenly under vacuum conditions to obtain the component A.
[0054] Step 2: Preparation of component B:
[0055] The preparation process of the degumming factor comprises the following steps:
[0056] (1) Heavy calcium and sodium bicarbonate are mixed in a mass ratio of 1:1 and added into a ball mill, and the grinding temperature is controlled to be ≤50°C and the humidity is ≤25% for grinding.
[0057] After grinding for a period of time, silane coupling agent is added several times for surface modification. The mass ratio of the total amount of silane coupling agent added to sodium bicarbonate is 1:100. Finally, composite particles of sodium bicarbonate and heavy calcium modified by silane coupling agent are obtained, and composite particles with a particle size of less than 20 μm are obtained by sieving.
[0058] Then, the material composition of the above-mentioned component B is added into a planetary mixer according to a weight ratio, and the component B is obtained after being dispersed and mixed evenly under vacuum conditions.
[0059] Step 3: Mixing of component A and component B: Mix components A and B evenly in a ratio of 1:1.3-1.4, apply it on the surface of one of the adherends, and connect the other adherend to it.
[0060] The difference between Example 2 to Example 6 and Example 1 is only the selection of some raw materials and process parameters, as shown in the table below. The mixing ratios of the components in Table 1 are all based on mass ratios.
[0061] Table 1 Addition amount: mass parts / g
[0062]
[0063]
[0064] Comparative Example 1
[0065] The difference between this comparative example and Example 2 is that no degumming factor is added in this comparative example.
[0066] Comparative Example 2
[0067] The difference between this comparative example and Example 2 is that in this comparative example, the degumming factor is replaced by mixed and ground sodium bicarbonate and heavy calcium mixed particles.
[0068] Comparative Example 3
[0069] The difference between this comparative example and Example 2 is that in this comparative example, the degumming factor is replaced by heavy calcium modified by a silane coupling agent.
[0070] Comparative Example 4
[0071] The difference between this comparative example and Example 2 is that in this comparative example, the degumming factor is replaced by sodium bicarbonate surface-modified with a silane coupling agent.
[0072] Experimental Example Performance Test
[0073] The adhesive sticks prepared in the above Examples 1-6 and Comparative Examples 1-4 were coated on silicon rods, and relevant data indicators were tested.
[0074] Hardness: The hardness test refers to GB / T 531.1-2008 "Test method for indentation hardness of vulcanized rubber or thermoplastic rubber" to test the hardness of the colloid after curing for 2 hours.
[0075] Adhesion and water resistance: Adhesion and water resistance are evaluated by pull-off force, referring to GB / T 5210-2006 "Pull-off adhesion test for paints and varnishes".
[0076] The mixed colloid was coated on the silicon wafer surface according to the test method requirements, cured for 2 hours, and the pull-out force of the colloid was evaluated. The sample cured for 2 hours was immersed in the cutting fluid for 24 hours, and the pull-out force after water resistance was tested.
[0077] The samples after curing for 2 h were immersed in aqueous lactic acid solutions at 20°C and 50°C for degumming test, and the degumming time was recorded.
[0078] The experiment was repeated three times for each group, and the results are shown in Table 2.
[0079] Table 2
[0080]
[0081] Table 3 Preparation of degumming factors in the embodiments and comparative examples and their dispersion in component B, wherein the mass of particles with a sieved particle size of less than 20 μm after grinding is ≥95%, which means that the grinding is uniform, and decomposition refers to the proportion of particle mass loss after grinding to sodium bicarbonate ≥2%, and whether there are particles in component B is observed by scraping glue on a glass plate.
[0082] Is the degumming factor ground evenly? Whether the degumming factor is decomposed by grinding Does component B have particles? Example 2 yes no no Comparative Example 1 -- -- no Comparative Example 2 yes no yes Comparative Example 3 yes no no Comparative Example 4 No, there is hardening yes no
[0083] The data of Examples 1-6 show that the epoxy adhesive stick of the present invention has the characteristics of high hardness, strong adhesion, good water resistance and rapid degumming at room temperature. After adding sodium bicarbonate and heavy calcium composite particles modified by silane coupling agent to the epoxy-polythiol epoxy adhesive stick system, the degumming time at 20°C is less than 15 minutes, and the degumming time at 20°C in Example 2 is only 7 minutes, which meets the degumming time requirements in the silicon wafer cutting process and meets the characteristics of rapid degumming at room temperature.
[0084] By comparing Example 2 with Comparative Example 1, it can be seen that the system without adding the degumming factor was not degummed after being soaked in 20°C acid solution for 1 hour. After raising the temperature to 50°C, the acid was boiled for 40 minutes for degumming, which could not meet the existing process requirements. The degumming factor in Comparative Example 2 was not modified by a silane coupling agent, resulting in uneven dispersion in the system, the presence of larger particles, affecting the performance, and increasing the chip drop rate. Only calcium carbonate was used as the degumming factor, and it was not degummed at 20°C for 1 hour, which did not meet the cutting process requirements. However, if only sodium bicarbonate was used, problems such as hardening and decomposition would easily occur during the grinding stage. In summary, the composite particles of sodium bicarbonate and heavy calcium modified by the silane coupling agent of the degumming factor in the system are the decisive factors for the rapid degumming of the colloid, and the compounding of sodium bicarbonate and heavy calcium can solve the problems of decomposition and hardening during the grinding process of sodium bicarbonate, and the modification of the silane coupling agent can solve the problem of aggregation of the degumming factor in the system and the generation of large particles.
[0085] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. An epoxy adhesive stick with rapid debonding at room temperature, characterized in that: The invention comprises component A and component B. Component A comprises the following raw materials in parts by mass: 30-70 parts of epoxy resin, 30-60 parts of filler, 0.01-2 parts of anti-settling agent, and 0.01-1 parts of defoaming agent; component B comprises the following raw materials in parts by mass: 20-70 parts of polythiol, 10-20 parts of degumming factor, 1-10 parts of accelerator, 0.05-2 parts of coupling agent, 20-60 parts of filler, 0.01-2 parts of anti-settling agent, and 0.01-1 parts of defoaming agent; the degumming factor is sodium bicarbonate and heavy calcium composite particles surface-modified by silane coupling agent; The preparation method of the degumming factor comprises the following steps: S1. Mix heavy calcium and sodium bicarbonate and grind them, wherein the mass ratio of heavy calcium to sodium bicarbonate is 1:1-5; S2. Add silane coupling agent for surface modification in multiple times, and the mass ratio of the total amount of silane coupling agent added to sodium bicarbonate is 1-5:
100.
2. The epoxy adhesive stick adhesive with rapid debonding at room temperature according to claim 1, characterized in that: The mass ratio of component A to component B is 1:0.5-2.
3. The epoxy adhesive stick adhesive with rapid debonding at room temperature according to claim 2, characterized in that: In step S1, the grinding conditions are temperature ≤ 50°C and humidity ≤ 25%.
4. The room temperature rapid debonding epoxy stick adhesive according to claim 3, characterized in that: In step S2, the surface is modified and then sieved to obtain composite particles of sodium bicarbonate and calcium carbonate modified by a silane coupling agent with a particle size of less than 20 μm.
5. The epoxy adhesive stick adhesive with rapid debonding at room temperature according to claim 4, characterized in that: The epoxy resin is at least one of E-20, E-44, E-51, E-54 and E-56; the filler is at least one of calcium carbonate, silicon powder, talcum powder, aluminum oxide, aluminum hydroxide and silicon dioxide; the anti-settling agent is at least one of fumed silica, organic bentonite and hydrogenated castor oil; the defoaming agent is at least one of 853, 554 and L-632.
6. The epoxy adhesive stick adhesive with rapid debonding at room temperature according to claim 5, characterized in that: The polythiol is at least one of R2000, R2020 and 830; the promoter is at least one of triethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, pyridine, resorcinol, m-cresol and phenol; and the coupling agent is at least one of KH550 and KH592.
7. A method for preparing an epoxy adhesive stick adhesive with rapid debonding at room temperature according to any one of claims 1 to 6, characterized in that: The steps include: Step 1: Preparation of component A: proportioning and mixing the materials of component A; Step 2, preparation of component B: using a silane coupling agent to modify the surface of sodium bicarbonate and heavy calcium to obtain degumming factor composite particles, and then proportioning and mixing the materials of component B; Step 3: Mixing component A and component B.
8. The method for preparing an epoxy adhesive stick adhesive with rapid debonding at room temperature according to claim 7, characterized in that: The mixing processes of step 1 and step 2 are both carried out under vacuum conditions.