Method for preparing lithium iron manganese phosphate positive electrode material using waste lithium iron phosphate batteries
Recover phosphorus iron resources from waste lithium iron phosphate batteries through high-temperature solid phase method, rationally add and coat them to prepare lithium iron manganese phosphate cathode materials, which solves the problems of low yield, high cost and environmental pollution in the existing technology, and achieves Preparation of high-performance and low-cost lithium iron manganese phosphate cathode materials.
Patent Information
- Application Number
- CN202310160196.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-20
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-02-20
AI Technical Summary
Existing methods for preparing lithium iron manganese phosphate have low technical yields, high costs, complex operations, are not suitable for mass production, and have environmental pollution problems.
Use high-temperature solid phase method to recover phosphorus iron resources from used lithium iron phosphate batteries, determine the element content through ICP detection, reasonably add manganese source, phosphorus source and lithium source, conduct ball milling and drying, and form non-stoichiometric lithium iron manganese phosphate. The carbon-coated lithium iron manganese phosphate cathode material is prepared by double-layer coating with sucrose and polyvinylidene fluoride-hexafluoropropylene copolymer, pre-sintering and sintering.
The preparation of low-cost, environmentally friendly lithium iron manganese phosphate cathode material has been achieved. The material has excellent performance, the discharge specific capacity reaches 147.6mAh/g, the electrochemical performance is improved, and no large amounts of organic solvents are used, which avoids environmental pollution.
Smart Images

Figure CN116143098B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of waste lithium iron phosphate battery resource recovery, and in particular to a method for preparing lithium iron manganese phosphate positive electrode materials by utilizing waste lithium iron phosphate batteries. Background Art
[0002] Lithium iron phosphate batteries have the advantages of low cost, high safety performance and good electrochemical cycle performance, and are widely used in the field of new energy vehicles. With the rapid development of the new energy field, the number of waste lithium iron phosphate batteries is also increasing. Therefore, the effective recycling and reuse of waste lithium iron phosphate batteries has both economic value and social benefits. Compared with lithium iron phosphate, lithium manganese iron phosphate (LiMn x Fe 1-x PO4, LMFP) has the advantages of higher working potential (Li+ / Li, 4.1V), greater energy density, longer cycle life, etc. At the same time, the price of lithium manganese iron phosphate resources is relatively low, and large-scale production can effectively reduce costs.
[0003] At present, the methods for preparing lithium iron manganese phosphate reported mainly include liquid phase method, high temperature solid phase method and spray drying method. For example, Chinese patent CN 115215315 uses hydrothermal method to recover iron and manganese from stainless steel slag to prepare lithium iron manganese phosphate. The hydrothermal method for preparing lithium iron manganese phosphate needs to be carried out under high temperature and high pressure, and a large amount of organic solvents need to be used, which will cause serious environmental pollution and is not suitable for mass production. At the same time, the content of iron and manganese elements in stainless steel slag is relatively low, and the yield of preparing lithium iron manganese phosphate using it is not high. Chinese patents CN 115231541 and CN111333049 publicly report the preparation of lithium iron manganese phosphate by spray drying method, but the equipment cost required for this method is relatively high and the operation is complicated. Summary of the invention
[0004] In order to solve the problems of low technical yield, high cost, complicated operation and inability to mass produce in existing methods for preparing lithium iron manganese phosphate, the present invention proposes a method for preparing lithium iron manganese phosphate positive electrode material using waste lithium iron phosphate batteries, and uses a high-temperature solid-phase method to recover phosphorus and iron resources from waste lithium iron phosphate batteries as raw materials to prepare lithium iron manganese phosphate. The present invention is reasonable, easy to implement, low-cost, environmentally friendly, and has high economic and social benefits.
[0005] The present invention is achieved through the following technical solution: a method for preparing lithium iron manganese phosphate positive electrode material using waste lithium iron phosphate batteries, the specific steps are as follows:
[0006] (1) Recovering ferrophosphorus residue from waste lithium iron phosphate batteries and determining the content of each element in the residue;
[0007] The conventional method is used to recover the ferrophosphorus residue from the waste lithium iron phosphate batteries, and then the ferrophosphorus residue recovered from the waste lithium iron phosphate batteries is subjected to ICP testing (inductively coupled plasma-emission spectroscopy testing) to determine the contents of elements such as phosphorus, iron, lithium and carbon in the residue.
[0008] (2) Based on lithium manganese iron phosphate Li y Mn x Fe 1-x The molar ratio of each element in PO4 is added to ferrophosphorus residue, manganese source, phosphorus source and lithium source, and then the mixture is placed in anhydrous ethanol medium for ball milling, and the obtained mixed powder is dried;
[0009] The ferrophosphorus residue and the manganese source, phosphorus source and lithium source can be prepared according to the molar ratio of the elements.
[0010] n(Li):n(Mn):n(Fe):n(P)=y:x:1-x:1 is added; and the ferrophosphorus residue is regarded as iron phosphate, and the non-stoichiometric lithium manganese iron phosphate is prepared by using the ferrophosphorus residue, in which the excess lithium will combine with the phosphate group to form lithium phosphate (Li3PO4), and the reaction mechanism is:
[0011] 3Li2CO3+2NH4H2PO4→2Li3PO4+2NH3↑+3CO2↑+3H2O↑
[0012] Supplementing excess lithium source, the formed Li3PO4 coating layer serves as a protective layer and ion conductor of lithium manganese iron phosphate, which can be used without sacrificing the interface Li + ions, provides a stable barrier coating for lithium manganese iron phosphate, which is beneficial to reduce the side reactions between the material and the electrolyte, thereby accelerating the transmission of lithium ions and improving the electrochemical properties of lithium manganese iron phosphate positive electrode materials.
[0013] Preferably, 0.5≤x≤0.7, wherein Li:P=y:1, 1<y≤1.3;
[0014] Preferably, the manganese source is selected from manganese carbonate (MnCO3), the lithium source is selected from lithium carbonate (Li2CO3), and the phosphorus source is selected from ammonium dihydrogen phosphate (NH4H2PO4).
[0015] Preferably, the ball milling rate is 400-600 r / min, and the ball milling time is 6-12 h.
[0016] Preferably, oven drying is adopted, the oven temperature is 80-120°C, and the drying time is 6-24h.
[0017] (3) pre-sintering the dried mixed powder;
[0018] Preferably, the dried mixture is placed in a tube furnace for pre-sintering;
[0019] Preferably, the pre-sintering is carried out in an inert gas atmosphere, the pre-sintering temperature is 350-450° C., the pre-sintering time is 6-8 hours, and the inert gas is preferably nitrogen or argon.
[0020] (4) adding sucrose and polyvinylidene fluoride-hexafluoropropylene copolymer P (VDF-HFP) to the pre-sintered mixture for a second layer coating, and ball milling in anhydrous ethanol medium, and drying to obtain a precursor;
[0021] Polyvinylidene fluoride-hexafluoropropylene copolymer P(VDF-HFP) is a derivative of PVDF. Its structural chemical properties are similar to those of PVDF, but P(VDF-HFP) contains more fluorine (F). The electronegativity of the F element is large, so adding a F-doped carbon coating is beneficial to reducing the charge transfer resistance. The F-doped carbon coating will form Mn-F bonds and CF covalent bonds at the interface, which helps to reduce the charge transfer resistance; and provide sufficient rapid electron transfer pathways.
[0022] Preferably, the added amount of sucrose and P(VDF-HFP) is 10wt% of the mixed powder in step (2), wherein the weight ratio of sucrose:P(VDF-HFP)=8:2.
[0023] In the preparation of lithium manganese iron phosphate, an excess lithium source is added, and the excess lithium reacts with the phosphate group to form Li3PO4 as the first layer coating of lithium manganese iron phosphate. Then a certain amount of sucrose and P(VDF-HFP) are added to the pre-sintered product. During the pyrolysis of P(VDF-HFP), some structural defects will appear, such as the infiltration of CF covalent bonds, topological defects, vacancies, etc. These structures are conducive to the storage of lithium and Li + and electron migration, thereby improving the electrochemical performance of lithium manganese iron phosphate.
[0024] Preferably, the ball milling speed is 450-650 r / min, and the ball milling time is 3-6 h.
[0025] (5) Sintering the precursor to obtain a double-layer coated lithium manganese iron phosphate positive electrode material.
[0026] Preferably, the sintering temperature is 550-750° C., and the sintering time is 12 h-15 h.
[0027] The present invention adopts a high-temperature solid phase method to prepare a carbon-coated lithium manganese iron phosphate material, and the 0.1C discharge specific capacity can reach 147.6 mAh / g, and the median discharge voltage is 3.95.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) Low cost, environmentally friendly, no large amount of organic solvent is used in the preparation process, and no waste liquid and residue that pollutes the environment are generated;
[0030] (2) The prepared double-layer coated lithium manganese iron phosphate material has uniform particle size and excellent material performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the XRD (X-ray diffraction analysis) diagram of the prepared lithium manganese iron phosphate;
[0032] Among them: (a) is the XRD of lithium iron manganese phosphate prepared from ferrophosphorus residue, (b) is the XRD of lithium iron manganese phosphate prepared with different lithium-phosphorus ratios;
[0033] Figure 2 The charge and discharge curve of the lithium iron manganese phosphate positive electrode material prepared in Example 2 of the present invention;
[0034] Figure 3 The charge and discharge curve of the lithium iron manganese phosphate positive electrode material prepared in Comparative Example 2 of the present invention;
[0035] Figure 4 The charge and discharge comparison curves of the lithium iron manganese phosphate positive electrode materials prepared in Comparative Example 1 and Example 2 of the present invention;
[0036] Figure 5 The charge and discharge comparison curves of the lithium iron manganese phosphate positive electrode materials prepared in comparative example 3 and example 2 of the present invention. DETAILED DESCRIPTION
[0037] The present invention is further described in detail below through specific examples and drawings. The raw materials used in the examples can be purchased from the market or prepared by conventional methods.
[0038] In this embodiment, the ferrophosphorus residue is derived from ferrophosphorus resources recovered from waste lithium iron phosphate batteries by sulfuric acid pickling, and is used as a raw material to replace conventional raw materials to prepare lithium iron manganese phosphate.
[0039] Example 1
[0040] (1) The molar ratio of phosphorus to iron in the ferrophosphorus residue measured by ICP is nearly 1:1.
[0041] (2) Press Li y Mn x Fe 1-xIn PO4, x=0.5, Li:P=1.15:1, n(Li):n(Mn):n(Fe):n(P)=1.15:0.5:0.5:1, lithium carbonate, lithium manganate, ferrophosphorus residue and ammonium dihydrogen phosphate are weighed and mixed, the mixed materials are placed in anhydrous ethanol medium for ball milling, and a mixed powder is obtained after drying, the ball milling rate is 400r / min, and the ball milling time is 6h; after ball milling, it is dried, the oven temperature is 100℃, and the drying time is 6h;
[0042] (3) placing the dried mixed material into a tubular furnace, introducing nitrogen, and pre-sintering at 350° C. for 6 h to obtain a pre-sintered product;
[0043] (4) 10 wt% of sucrose and P (VDF-HFP) in the mixed powder in step (2), wherein the weight ratio of sucrose to P (VDF-HFP) is 8:2, is added to the product obtained after pre-sintering, and ball milled in anhydrous ethanol medium for double-layer coating to obtain a precursor, the ball milling speed is 500 r / min, and the ball milling time is 3 h;
[0044] (5) The coated precursor was placed in a tube furnace, nitrogen was introduced, and sintered at 650° C. for 12 h to obtain a double-layer coated lithium manganese iron phosphate positive electrode material 1.
[0045] Example 2
[0046] (1) The molar ratio of phosphorus to iron in the ferrophosphorus residue measured by ICP is nearly 1:1;
[0047] (2) Press Li y Mn x Fe 1-x In PO4, x=0.6, Li:P=1.15:1, and the molar ratio of n(Li):n(Mn):n(Fe):n(P)=1.15:0.6:0.4:1. Lithium carbonate, lithium manganate, ferrophosphorus residue and ammonium dihydrogen phosphate are weighed and mixed. The mixed materials are placed in anhydrous ethanol medium for ball milling. After drying, a mixed powder is obtained. The ball milling rate is 400 r / min and the ball milling time is 6 h. After ball milling, the mixture is dried at an oven temperature of 100°C and the drying time is 6 h.
[0048] (3) placing the dried mixed material into a tubular furnace, introducing nitrogen, and pre-sintering at 350° C. for 6 h to obtain a pre-sintered product;
[0049] (4) taking 10 wt% of sucrose and P(VDF-HFP) in the mixed powder in step (2), wherein the weight ratio of sucrose to P(VDF-HFP) is 8:2, adding it to the product obtained after pre-sintering, and ball milling it in anhydrous ethanol medium for double-layer coating to obtain a precursor, the ball milling speed is 500 r / min, and the ball milling time is 3 h;
[0050] (5) The coated precursor was placed in a tube furnace, nitrogen was introduced, and sintered at 650° C. for 12 h to obtain a double-layer coated lithium manganese iron phosphate positive electrode material 2.
[0051] Example 3
[0052] (1) The molar ratio of phosphorus to iron in the ferrophosphorus residue measured by ICP is nearly 1:1;
[0053] (2) Press Li y Mn x Fe 1-x In PO4, x=0.6, Li:P=1.3:1, n(Li):n(Mn):n(Fe):n(P)=1.3:0.6:0.4:1, lithium carbonate, lithium manganate, ferrophosphorus residue and ammonium dihydrogen phosphate are weighed and mixed, the mixed materials are placed in anhydrous ethanol medium for ball milling, and a mixed powder is obtained after drying, the ball milling rate is 400r / min, and the ball milling time is 6h; after ball milling, it is dried, the oven temperature is 100℃, and the drying time is 6h;
[0054] (3) placing the dried mixed material into a tubular furnace, introducing nitrogen, and pre-sintering at 350° C. for 6 h to obtain a pre-sintered product;
[0055] (4) taking 10 wt% of sucrose and P(VDF-HFP) in the mixed powder in step (2), wherein the weight ratio of sucrose to P(VDF-HFP) is 8:2, adding it to the product obtained after pre-sintering, and ball milling it in anhydrous ethanol medium for double-layer coating to obtain a precursor, the ball milling speed is 500 r / min, and the ball milling time is 3 h;
[0056] (5) The double-layer coated precursor was placed in a tube furnace, nitrogen was introduced, and sintered at 650° C. for 12 h to obtain a carbon-coated lithium manganese iron phosphate positive electrode material 3.
[0057] Comparative Example 1: Only sucrose was added
[0058] (1) The molar ratio of phosphorus to iron in the ferrophosphorus residue measured by ICP is nearly 1:1;
[0059] (2) Press Li y Mn x Fe 1-xIn PO4, x=0.6, Li:P=1.15:1, n(Li):n(Mn):n(Fe):n(P)=1.15:0.6:0.4:1, lithium carbonate, lithium manganate, ferrophosphorus residue and ammonium dihydrogen phosphate are weighed and mixed, the mixed materials are placed in anhydrous ethanol medium for ball milling, and a mixed powder is obtained after drying, the ball milling rate is 400r / min, and the ball milling time is 6h; after ball milling, it is dried, the oven temperature is 100℃, and the drying time is 6h;
[0060] (3) placing the dried mixed material into a tubular furnace, introducing nitrogen, and pre-sintering at 350° C. for 6 h to obtain a pre-sintered product;
[0061] (4) adding 10 wt% sucrose from the mixed powder in step (2) to the product obtained after pre-sintering, and ball milling in anhydrous ethanol medium for double-layer coating to obtain a precursor, the ball milling speed is 500 r / min, and the ball milling time is 3 h;
[0062] (5) The double-layer coated precursor was placed in a tube furnace, nitrogen was introduced, and sintered at 650° C. for 12 h to obtain a carbon-coated lithium manganese iron phosphate positive electrode material 4.
[0063] Comparative Example 2: y = 1
[0064] (1) The molar ratio of phosphorus to iron in the ferrophosphorus residue measured by ICP is nearly 1:1.
[0065] (2) Press Li y Mn x Fe 1-x In PO4, x=0.6, Li:P=1:1, n(Li):n(Mn):n(Fe):n(P)=1:0.6:0.4:1, lithium carbonate, lithium manganate, ferrophosphorus residue and ammonium dihydrogen phosphate are weighed and mixed, the mixed materials are placed in anhydrous ethanol medium for ball milling, and a mixed powder is obtained after drying, the ball milling rate is 400r / min, and the ball milling time is 6h; after ball milling, it is dried, the oven temperature is 100℃, and the drying time is 6h;
[0066] (3) placing the dried mixed material into a tubular furnace, introducing nitrogen, and pre-sintering at 350° C. for 6 h to obtain a pre-sintered product;
[0067] (4) 10 wt% of sucrose and P (VDF-HFP) in the mixed powder in step (2), wherein the weight ratio of sucrose to P (VDF-HFP) is 8:2, is added to the product obtained after pre-sintering, and ball milled in anhydrous ethanol medium for double-layer coating to obtain a precursor, the ball milling speed is 500 r / min, and the ball milling time is 3 h;
[0068] (5) The coated precursor was placed in a tube furnace, nitrogen was introduced, and sintered at 650° C. for 12 h to obtain a double-layer coated lithium manganese iron phosphate positive electrode material 5.
[0069] Comparative Example 3: Sucrose and P(VDF-HFP) added in an amount exceeding 10 wt%
[0070] (1) The molar ratio of phosphorus to iron in the ferrophosphorus residue measured by ICP is nearly 1:1;
[0071] (2) Press Li y Mn x Fe 1-x In PO4, x=0.6, Li:P=1.15:1, n(Li):n(Mn):n(Fe):n(P)=1.15:0.6:0.4:1, lithium carbonate, lithium manganate, ferrophosphorus residue and ammonium dihydrogen phosphate are weighed and mixed, the mixed materials are placed in anhydrous ethanol medium for ball milling, and a mixed powder is obtained after drying, the ball milling rate is 400r / min, and the ball milling time is 6h; after ball milling, it is dried, the oven temperature is 100℃, and the drying time is 6h;
[0072] (3) placing the dried mixed material into a tubular furnace, introducing nitrogen, and pre-sintering at 350° C. for 6 h to obtain a pre-sintered product;
[0073] (4) taking 20 wt% of sucrose and P(VDF-HFP) in the mixed powder in step (2), wherein the weight ratio of sucrose to P(VDF-HFP) is 8:2, adding it to the product obtained after pre-sintering, and ball milling in anhydrous ethanol medium for double-layer coating to obtain a precursor, the ball milling speed is 500 r / min, and the ball milling time is 3 h;
[0074] (5) The double-layer coated precursor was placed in a tube furnace, nitrogen was introduced, and sintered at 650° C. for 12 h to obtain a carbon-coated lithium manganese iron phosphate positive electrode material 6.
[0075] Test Example 1
[0076] X-ray diffraction analysis was performed on the positive electrode materials and ferrophosphorus residue of lithium manganese iron phosphate prepared in the examples and comparative examples. The test results are as follows: Figure 1 As shown. (a) is LiMn 0.6 Fe 0.4 PO4 and residue were analyzed by X-ray diffraction. It can be clearly seen that the sample has good crystallization performance, and all diffraction peaks match the diffraction peaks of the standard olivine structure (pnmb space group, JCPDS 74-0375), as shown in PDF#74-0375. No other obvious impurity peaks were found, indicating that a pure olivine phase was formed. At the same time, it can be found that some diffraction peaks are shifted to high angles. This is due to the Fe2+ The ionic radius Less than Mn 2+ The ionic radius When Fe 2+ Replace part of Mn 2+ As a result, the unit cell volume is reduced. From the (b) XRD graph, it can be seen that when 1<y≤1.3, there is a diffraction peak of Li3PO4 at 2θ≈23°, where the higher the lithium content, the stronger the corresponding diffraction peak intensity; Li3PO4 exists in the form of a second phase and has a higher lithium ion diffusion coefficient; this is beneficial to improving the electrochemical performance of the positive electrode material.
[0077] Test Example 2
[0078] The positive electrode materials of lithium iron manganese phosphate prepared in Example 2 and Comparative Example 2 were subjected to charge and discharge tests. The charge and discharge curves of the positive electrode materials of lithium iron manganese phosphate prepared in Example 2 and Comparative Example 2 are shown in Figure 2. Figure 2 , Figure 3 As shown;
[0079] The corresponding discharge capacity at 0.1C rate is 125.8mAh / g, 151.8mAh / g, and 149.8mAh / g. From Table 1, it can be seen that the discharge capacity of lithium iron manganese phosphate is obviously improved by the excess lithium.
[0080] Table 1
[0081] <![CDATA[Li y Mn x Fe 1-x PO4]]> Li:P molar ratio 0.1C discharge capacity mAh / g 0.1C discharge median voltage Comparative Example 2 1:1 125.8 3.59 Example 2 1.15:1 151.8 3.97 Example 3 1.3:1 149.8 3.94
[0082] like Figure 4 As shown, at 1C, the discharge specific capacity of LMFP / CF in Example 2 is 147.6 mAh / g, which is slightly higher than the discharge specific capacity (144.8 mAh / g) of LMFP / C in Comparative Example 1. The anode peak profile of LMFP / CF is sharper and more symmetrical than that of LMFP / C, indicating that it has better ion transport capability.
[0083] like Figure 5 As shown, at 1C, the discharge specific capacity of the lithium iron manganese phosphate with sucrose and P (VDF-HFP) added in an amount of 20wt% in Comparative Example 3 is 141.3mAh / gd, which is lower than the discharge specific capacity of the lithium iron manganese phosphate with sucrose and P (VDF-HFP) added in an amount of 10wt%; this is mainly because when too much sucrose is added, the carbon coating layer will hinder lithium ions and reduce the conductivity of the lithium iron manganese phosphate.
Claims
1. A method for preparing lithium iron manganese phosphate positive electrode material using waste lithium iron phosphate batteries, characterized in that: The preparation method comprises the following steps: (1) Recovering ferrophosphorus waste residue from waste lithium iron phosphate batteries and determining the content of each element in the waste residue; (2) Based on lithium manganese iron phosphate Li y Mn x Fe 1-x The molar ratio of each element in PO4 is added to ferrophosphorus residue, manganese source, phosphorus source and lithium source, and then the mixture is ball-milled in anhydrous ethanol medium and dried to obtain a mixed powder; (3) pre-sintering the dried mixed powder; (4) adding sucrose and polyvinylidene fluoride-hexafluoropropylene copolymer to the pre-sintered mixture for a second layer coating, and ball milling in anhydrous ethanol medium, and drying to obtain a precursor; (5) Sintering the precursor to obtain a double-layer coated lithium manganese iron phosphate positive electrode material.
2. The method for preparing lithium iron manganese phosphate positive electrode material using waste lithium iron phosphate batteries according to claim 1, characterized in that: In step (2), the manganese source is selected from manganese carbonate, the lithium source is selected from lithium carbonate, and the phosphorus source is selected from ammonium dihydrogen phosphate.
3. A method for preparing lithium iron manganese phosphate positive electrode material using waste lithium iron phosphate batteries according to claim 1 or 2, characterized in that: In step (2), 0.5≤x≤0.7, 1<y≤1.
3.
4. The method for preparing lithium iron manganese phosphate positive electrode material using waste lithium iron phosphate batteries according to claim 1, characterized in that: In step (2), the ball milling rate is 400-600 r / min, and the ball milling time is 6-12 h.
5. The method for preparing lithium iron manganese phosphate positive electrode material using waste lithium iron phosphate batteries according to claim 1, characterized in that: Step (2) is dried in an oven at a temperature of 80-120° C. for a drying time of 6-24 hours.
6. The method for preparing lithium iron manganese phosphate positive electrode material using waste lithium iron phosphate batteries according to claim 1, characterized in that: Step (3) is to perform pre-sintering in an inert gas atmosphere, the pre-sintering temperature is 350-450° C., and the pre-sintering time is 6-8 hours.
7. The method for preparing lithium iron manganese phosphate positive electrode material using waste lithium iron phosphate batteries according to claim 1, characterized in that: In step (4), the amount of sucrose and polyvinylidene fluoride-hexafluoropropylene copolymer added is 10% of the weight of the mixed powder in step (2).
8. The method for preparing lithium iron manganese phosphate positive electrode material using waste lithium iron phosphate batteries according to claim 7, characterized in that: The weight ratio of sucrose to polyvinylidene fluoride-hexafluoropropylene copolymer is 8:
2.
9. The method for preparing lithium iron manganese phosphate positive electrode material using waste lithium iron phosphate batteries according to claim 1, characterized in that: In step (4), the ball milling speed is 450-650 r / min, and the ball milling time is 3-6 h.
10. The method for preparing lithium iron manganese phosphate positive electrode material using waste lithium iron phosphate batteries according to claim 1, characterized in that: In step (5), the sintering temperature is 550-750° C. and the sintering time is 12 h-15 h.
Citation Information
Patent Citations
Preparation method of lithium iron manganese phosphate cathode composite material
CN102738465A