Conductive ink for copper-nickel alloy electrode, substrate with copper-nickel alloy electrode, and method for producing the same
By controlling the nickel content and combining copper particles in the conductive ink for copper-nickel alloy electrodes, the problems of high stability and cost of copper-nickel alloy electrodes in the prior art are solved, and cheap and atmospheric stability are achieved Excellent metal wiring for wearable devices.
Patent Information
- Application Number
- CN202180068292.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-15
- Filing Date
- 2021-11-19
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-11-19
AI Technical Summary
The existing copper-silver alloy electrode inks have problems such as insufficient stability, high cost and expensiveness in materials in practical use, and the problems of high sintering temperature and high cost of copper-nickel alloy electrodes have not been effectively solved.
Using conductive ink for copper-nickel alloy electrodes containing specific copper complexes and nickel complexes, the nickel content is controlled in the range of more than 5% and less than 80% in the total mass of copper and nickel. The use of particles is used to form a copper-nickel alloy, and the coating method is adopted, and the substrate is heated at 170°C to 250°C.
Inexpensive and excellent atmospheric stability are achieved, and copper-nickel alloy electrodes with smooth surfaces without cracks are obtained, suitable for wearable devices and reduce the cost of the electrodes.
Smart Images

Figure CN116323044B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a conductive ink for a copper-nickel alloy electrode, a substrate with a copper-nickel alloy electrode, and a method for producing the same. Background Art
[0002] In recent years, printed electronic circuits have been developed as a wiring technology for semiconductor devices, electronic circuits, etc. Printed electronic circuits have attracted attention because they can reduce manufacturing costs compared to existing semiconductor manufacturing technologies such as photolithography.
[0003] As ink for such printed electronic circuits, ink using a complex has been developed (for example, refer to non-patent document 1 and non-patent document 2). According to non-patent document 1, by using copper particles and silver complexes, a metal wiring having a core-shell structure in which copper particles are coated with a copper-silver alloy can be obtained. According to non-patent document 2, by using copper complexes and silver complexes, a metal wiring composed of a copper-silver alloy can be obtained. In either case, by forming a copper-silver alloy, the oxidation resistance is improved compared to that of pure copper metal wiring, but further improvement is required in practical application. In addition, bumps, lumps, and cracks will occur on the electrode during use, and the stability is also insufficient. In addition, the material becomes expensive due to the presence of silver.
[0004] Since nickel particles are chemically more stable than copper particles and cheaper than silver particles, they are also used in electrodes (for example, see Patent Document 1). According to Patent Document 1, it is disclosed that nickel particles can be obtained from a nickel complex obtained from nickel formate dihydrate and an aliphatic amine, and it is reported that the particle size of the nickel particles can be controlled by changing the alkyl chain length of the aliphatic amine.
[0005] Copper nanoparticles having a nickel-copper alloy on the surface have been developed (for example, see Patent Document 2). According to Patent Document 2, oxidation resistance is improved by the nickel-copper alloy on the surface, and the nanoparticles are used for fine wiring by printing or coating. However, even if such copper nanoparticles are used, there are still problems that the ink stability is still insufficient to reach a practical level, and the firing temperature is high and the cost is high.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2010-064983.
[0009] Patent document 2: Japanese Patent Application Publication No. 2011-063828.
[0010] Non-patent literature
[0011] Non-patent literature 1: Wanli Li et al., ACS Appl. Mater. Interfaces, 2017, 9, 24711-24721.
[0012] Non-patent document 2: Wanli Li et al., Nanoscale, 2018, 10, 5254. Summary of the invention
[0013] Problems to be solved by the invention
[0014] As described above, the present invention aims to provide a conductive ink for copper-nickel alloy electrodes which is inexpensive, has excellent atmospheric stability, and can provide metal wiring with a smooth surface, a substrate with copper-nickel alloy electrodes, and a method for producing the same.
[0015] Means for solving problems
[0016] The conductive ink for copper-nickel alloy electrodes of the present invention contains a copper complex represented by general formula A and a nickel complex represented by general formula B, and the content ratio of nickel is in the range of 5 mass % or more and less than 80 mass % relative to the total mass of copper and nickel, thereby solving the above-mentioned problems.
[0017] Cu(HCOO)2(L 1 ) m A
[0018] Ni(HCOO)2(L 2 ) n B
[0019] Here, m and n are natural numbers from 2 to 6, respectively. 1 are the same or different amino alcohols having one amino group, L 2 They are the same or different aliphatic amines having one amino group, or vice versa.
[0020] The amino alcohol may have one primary amino group, at least one hydroxyl group, and a saturated or unsaturated linear, branched, or cyclic hydrocarbon group having 1 to 20 carbon atoms.
[0021] The amino alcohol may be selected from 2-aminoethanol, 2-amino-2-methyl-1-propanol, 1-amino-2-propanol, 2-amino-1-propanol, 1-amino-2-methyl-2-propanol, 2-amino-1-butanol, 1-amino-2-butanol, 2-amino-3,3-dimethyl-1-butanol, 2-amino-3-methyl-1-butanol, 2-amino-4-methyl-1-pentanol, 3-amino-1-propanol, 5-amino-1-pentanol, 6-amino-1-butanol, 7-amino-2-methyl-2-propanol, 8-amino-1-butanol, 10-amino-2-butanol, 11-amino-2-butanol, 12-amino-2-butanol, 13-amino-2-butanol, 14-amino-2-butanol, 15-amino-2-butanol, 16-amino-2-butanol, 17-amino-2-butanol, 18-amino-2-butanol, 19-amino-2-butanol, 20-amino-2-butanol, 21-amino-2-butanol, 23-amino-2-butanol, 24-amino-2-methyl-1-pentanol, 24-amino-2-butanol, 25-amino-2-butanol, 26-amino-2-butanol, 27-amino-2-butanol, 28-amino-2 The invention can be selected from the group consisting of: -hexanol, 3-amino-2,2-dimethyl-1-propanol, 4-amino-1-butanol, 8-amino-1-octanol, 10-amino-1-decanol, 12-amino-1-dodecanol, 2-aminocyclohexanol, 4-amino-2-methyl-1-butanol, 2-amino-1,3-propanediol, 2-amino-2-methyl-1,3-propanediol, 3-amino-1,2-propanediol and 2-amino-2-ethyl-1,3-propanediol.
[0022] The aliphatic amine may have one primary amino group and a saturated or unsaturated linear, branched or cyclic hydrocarbon group having 1 to 20 carbon atoms.
[0023] The aliphatic amine may be selected from the group consisting of 2-ethylhexylamine, n-butylamine, tert-butylamine, benzylamine, n-hexylamine, 2-heptylamine, cyclohexylamine and n-dodecylamine.
[0024] The nickel content may be in the range of 10 mass % or more and 70 mass % or less.
[0025] The nickel content may be in the range of 19 mass % or more and 67 mass % or less.
[0026] The conductive ink may further contain copper particles and / or nickel particles.
[0027] The conductive ink may further contain a monohydric alcohol and / or a polyhydric alcohol.
[0028] The monohydric alcohol may be selected from the group consisting of methanol, ethanol, 1-propanol, 1-butanol, 2-butanol, 2-methyl-1-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 3-methyl-1-butanol, 2-methyl-1-butanol, 2,2-dimethyl-1-propanol, 3-methyl-2-butanol and 2-methyl-2-butanol.
[0029] The polyol may be selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, butylene glycol, pentylene glycol, dipropylene glycol, tripropylene glycol, polyethylene glycol, polypropylene glycol and glycerol.
[0030] The method for producing the conductive ink of the present invention comprises: 1The amine ligand represented by is mixed to form a copper complex; nickel formate is mixed with L 2 The amine ligand represented by is mixed to form a nickel complex; and the copper complex and the nickel complex are mixed in such a way that the mass ratio of the nickel complex to the copper complex satisfies 0.05 or more and less than 6. 1 are the same or different amino alcohols having one amino group, wherein L 2 The above-mentioned problems can be solved by using the same or different aliphatic amines having one amino group, or the opposite.
[0031] In the formation of the nickel complex, a polyol may be further mixed.
[0032] The polyol may be selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, butylene glycol, pentylene glycol, dipropylene glycol, tripropylene glycol, polyethylene glycol, polypropylene glycol and glycerol.
[0033] During the mixing, a monohydric alcohol may be further added.
[0034] During the mixing, copper particles and / or nickel particles may be further mixed.
[0035] The substrate with a copper-nickel alloy electrode of the present invention comprises a substrate and an electrode containing a copper-nickel alloy located on the substrate, wherein the content ratio of nickel in the copper-nickel alloy relative to the total mass of copper and nickel is in the range of 5 mass % or more and less than 80 mass %, thereby solving the above-mentioned problem.
[0036] The substrate may be selected from the group consisting of polyethylene naphthalate, polyimide, and polyolefin resin.
[0037] The method of manufacturing a substrate with a copper-nickel alloy electrode of the present invention comprises applying the above-mentioned conductive ink to a substrate, and heating the substrate applied with the conductive ink, thereby solving the above-mentioned problem.
[0038] The coating may be performed by a method selected from the group consisting of spin coating, spray coating, dip coating, slit coating, slot coating, rod coating, roll coating, curtain coating, gravure printing, inkjet and screen printing.
[0039] The heating may be performed at a temperature ranging from 170° C. to 250° C. and for a time ranging from 1 minute to 60 minutes.
[0040] The above method may further include heating by light irradiation after the heating.
[0041] Effects of the Invention
[0042] The conductive ink for copper-nickel alloy electrodes of the present invention contains the copper complex represented by the general formula A and the nickel complex represented by the general formula B, and the content of nickel is in the range of 5 mass % or more and less than 80 mass % relative to the total mass of copper in the copper complex and nickel in the nickel complex. By containing specific copper complexes and nickel complexes, the generation of copper oxide is suppressed and the formation of copper-nickel alloy is promoted, and the conductive ink is inexpensive and has excellent atmospheric stability. In addition, by controlling the nickel content within the above range, a smooth and crack-free metal wiring can be obtained.
[0043] In addition, since the copper-nickel alloy can be easily formed at a low temperature by using the conductive ink for copper-nickel alloy electrodes of the present invention, a polymer substrate with a copper-nickel alloy electrode can be provided, which can be applied to wearable devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 1 is a flow chart showing the process of producing the conductive ink of the present invention.
[0045] Figure 2 This is a schematic diagram showing a substrate with a copper-nickel alloy electrode according to the present invention.
[0046] Figure 3 This is a flow chart showing the steps of manufacturing the substrate with copper-nickel alloy electrodes according to the present invention.
[0047] Figure 4 This is a diagram showing the appearance of the electrode of Example 1.
[0048] Figure 5 The figures show optical microscope photographs of the electrodes of Examples 1 to 6.
[0049] Figure 6 The figures show optical microscope photographs of the electrodes of Examples 7 to 10.
[0050] Figure 7 This is a diagram showing a SEM image of the electrode of Example 1.
[0051] Figure 8 This is a diagram showing the EDS element distribution of the electrode of Example 1.
[0052] Fig. 9 The figures show SEM images of the electrodes of Examples 7 to 9.
[0053] Fig.10 The diagram shows SEM images of the electrodes of Examples 17 and 18.
[0054] Fig.11 It is a figure which shows the XRD spectrum of the electrode of Example 1 - Example 4.
[0055] Fig.12 This is a graph showing the resistance of the electrodes of Examples 1 to 4.
[0056] Fig.13 This is a graph showing the dependence of the resistance of the electrode on the nickel content ratio.
[0057] Fig.14 It is a graph showing the results of the oxidation resistance test. DETAILED DESCRIPTION
[0058] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. It should be noted that the same elements are denoted by the same reference numerals and their description will be omitted.
[0059] (Implementation Method 1)
[0060] In the first embodiment, the conductive ink for copper-nickel alloy electrodes and the method for producing the conductive ink according to the present invention are described.
[0061] The conductive ink for copper-nickel alloy electrodes of the present invention (hereinafter, simply referred to as conductive ink) contains a copper complex represented by the general formula A and a nickel complex represented by the general formula B.
[0062] Cu(HCOO)2(L 1 ) m A
[0063] Ni(HCOO)2(L 2 ) n B
[0064] Here, m and n are natural numbers from 2 to 6, respectively. 1 and L 2 is an amine ligand. Specifically, L 1 are the same or different amino alcohols having one amino group, L 2 are the same or different aliphatic amines having one amino group, or vice versa, i.e., L 1 are the same or different aliphatic amines having one amino group, L 2 The amino alcohols are the same or different amino alcohols having one amino group. Since the combination of the amino alcohol and the aliphatic amine can obtain a copper-nickel alloy in the heat treatment after coating, it is possible to provide a stable metal wiring having excellent oxidation resistance.
[0065] In addition, in the conductive ink of the present invention, the content of nickel is within the range of 5 mass % or more and less than 80 mass % relative to the total mass of copper and nickel contained. When the content of nickel is less than 5 mass %, the surface is uneven and smooth metal wiring cannot be obtained. When the content of nickel is 80 mass % or more, the copper-nickel alloy is cracked and the resistance is increased, so it cannot function as an electrode.
[0066] As L 1The amino alcohol having one amino group, preferably one primary amino group, at least one hydroxyl group, and a saturated or unsaturated straight chain, branched or cyclic hydrocarbon group having 1 to 20 carbon atoms. By having a primary amino group, it coordinates and complexes with copper ions. By having one or more hydroxyl groups, the affinity with the nickel complex is excellent. When the number of carbon atoms is 1 to 20, a copper-nickel alloy can be obtained. From the viewpoint of affinity with the nickel complex and promotion of copper-nickel alloy formation, the number of carbon atoms is more preferably 2 to 10, and further preferably 2 to 5. L 1 The compounds may be the same or different, but are preferably the same from the viewpoint of yield.
[0067] As the amino alcohol having one amino group, in the manufacture of ink using existing copper nanoparticles, an amino alcohol used in forming a copper complex can be applied. Preferably, the amino alcohol having one amino group is selected from 2-aminoethanol, 2-amino-2-methyl-1-propanol, 1-amino-2-propanol, 2-amino-1-propanol, 1-amino-2-methyl-2-propanol, 2-amino-1-butanol, 1-amino-2-butanol, 2-amino-3,3-dimethyl-1-butanol, 2-amino-3-methyl-1-butanol, 2-amino-4-methyl-1-pentanol, 3-amino-1-propanol, 5-amino-1-pentanol, 6-amino-1-butanol, 7-amino-2-methyl-2-propanol, 8-amino-1-butanol, 10-amino-2-butanol, 11-amino-2-butanol, 12-amino-2-butanol, 13-amino-2-butanol, 14-amino-2-methyl-2-propanol, 15-amino-2-butanol, 16-amino-2-methyl-2-propanol, 17-amino-2-butanol, 18-amino-2-butanol, 19-amino-3-methyl-1-butanol, 20-amino-3-methyl-1-butanol, 21-amino-3-methyl-1-pentanol, 22-amino-3-methyl-1-pentanol, 23-amino-4-methyl-1-pentanol, 24-amino-3-propanol, 25-amino-3-pentanol, 26-amino-3-pentanol, 27-amino-3-pentanol, 28-amino-3-pentanol, 29-amino-4-methyl-1-pentanol, 30-amino The present invention can be selected from the group consisting of 1-aminohexanol, 3-amino-2,2-dimethyl-1-propanol, 4-amino-1-butanol, 8-amino-1-octanol, 10-amino-1-decanol, 12-amino-1-dodecanol, 2-aminocyclohexanol, 4-amino-2-methyl-1-butanol, 2-amino-1,3-propanediol, 2-amino-2-methyl-1,3-propanediol, 3-amino-1,2-propanediol and 2-amino-2-ethyl-1,3-propanediol. These are easily available and promote the formation of copper complexes.
[0068] As L 2 An aliphatic amine having one amino group, a primary amino group, and a saturated or unsaturated straight chain, branched or cyclic hydrocarbon group having 1 to 20 carbon atoms. By having a primary amino group, it coordinates and complexes with nickel ions. When the number of carbon atoms is 1 to 20, a copper-nickel alloy can be obtained. From the viewpoint of affinity with copper complexes and promotion of copper-nickel alloy formation, the number of carbon atoms is more preferably 2 to 10, and further preferably 2 to 7. 2 The compounds may be the same or different, but are preferably the same from the viewpoint of yield.
[0069] The aliphatic amine having one amino group is preferably selected from the group consisting of 2-ethylhexylamine, n-butylamine, tert-butylamine, benzylamine, n-hexylamine, 2-heptylamine, cyclohexylamine and n-dodecylamine. These are easily available and promote the formation of the nickel complex.
[0070] It should be noted that as L 2 Some of the above-mentioned aliphatic amines may have a hydroxyl group and may be an amino alcohol. In this case, the amino alcohol may be the above-mentioned amino alcohol.
[0071] In addition, as long as L 1 and L 2 It is a combination of the above amino alcohol and aliphatic amine, and it can also be L 2 For amino alcohol, L 1 is an aliphatic amine. In the present invention, by satisfying this combination, a copper-nickel alloy is formed to form a smooth metal wiring. It should be noted that even in L 1 In the case of aliphatic amines, some of the aliphatic amines may have hydroxyl groups, and for example, the above-mentioned amino alcohols may be used.
[0072] The coordination form of the formate ion in the copper formate of the general formula A and the nickel formate of the general formula B is easily determined by the ligand L used. 1 and L 2 Therefore, the range of m and n can be greater than 2 and less than 6. For example, in the general formula A, in the case where L 1 When 2-amino-2-methyl-1-propanol (AMP) is selected, it is bidentate coordination, m is 2, and in the general formula B, in the case of L 2 When 2-amino-2-methyl-1-propanol (AMP) is selected, it is a tetradentate coordination, and n is 4. A person skilled in the art will easily understand the change of such coordination number. The range of m and n is preferably greater than 2 and less than 4. Therefore, since the metal content in the conductive ink increases, it is preferred.
[0073] In the conductive ink of the present invention, the content of nickel relative to the total mass of copper and nickel preferably satisfies the range of 10 mass % to 70 mass %. Within this range, a metal wiring with few surface irregularities and smoothness can be obtained. The content of nickel further preferably satisfies the range of 19 mass % to 67 mass %. Within this range, a metal wiring with very few surface irregularities and very smoothness can be obtained. The content of nickel is particularly preferably in the range of 30 mass % to 50 mass %. Within this range, a metal wiring with oxidation resistance, very few surface irregularities, and very smoothness can be obtained.
[0074] The conductive ink of the present invention preferably further contains copper particles and / or nickel particles. Thus, thick metal wiring with a thickness of several μm or more can be obtained. The particle size of these particles is preferably in the range of 50 nm to 1 μm, more preferably in the range of 50 nm to 400 nm. Thus, thick metal wiring with few surface irregularities and no cracks can be obtained.
[0075] When copper particles are further contained, the copper particles may be contained in a manner such that the nickel content ratio relative to the total mass of copper and nickel satisfies the above range. Thus, a thick metal wiring with excellent coating properties, few surface irregularities, and no cracks can be obtained. The same is true for nickel particles. The same is true for the case of containing these two particles.
[0076] The conductive ink of the present invention may further contain a monohydric alcohol and / or a polyhydric alcohol. This allows the viscosity to be adjusted and the copper complex and the nickel complex to be uniformly mixed, thereby providing an ink having excellent coating properties.
[0077] The monohydric alcohol is preferably an alkyl alcohol, alkenyl alcohol or cycloalkyl alcohol having 5 or less carbon atoms, and specifically includes methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 3-methyl-1-butanol, 2-methyl-1-butanol, 2,2-dimethyl-1-propanol, 3-methyl-2-butanol, 2-methyl-2-butanol, cyclopropanol, cyclobutanol, cyclopentanol, etc. The monohydric alcohol is preferably selected from the group consisting of methanol, ethanol, 1-propanol, 1-butanol, 2-butanol, 2-methyl-1-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 3-methyl-1-butanol, 2-methyl-1-butanol, 2,2-dimethyl-1-propanol, 3-methyl-2-butanol and 2-methyl-2-butanol. These are easily available and have a boiling point of 150° C. or lower, and are therefore suitable for adjusting the viscosity.
[0078] The polyol may be a diol or a triol. The polyol is preferably selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, butanediol, pentanediol, dipropylene glycol, tripropylene glycol, polyethylene glycol, polypropylene glycol and glycerol. These are easily available and form a conductive ink in which the copper complex and the nickel complex are uniformly mixed.
[0079] The viscosity of the conductive ink can be appropriately adjusted depending on the application. For example, when the conductive ink is used for inkjet printing, a monohydric alcohol and / or a polyhydric alcohol may be added so that the viscosity of the conductive ink is 1 mPa·s or more and 20 mPa·s or less.
[0080] Next, an exemplary method for producing the conductive ink for copper-nickel alloy electrodes of the present invention will be described.
[0081] Figure 1 1 is a flow chart showing the process of producing the conductive ink of the present invention.
[0082] Step S110: Copper formate and L 1 The amine ligand represented by L is mixed to form a copper complex. 1 The copper complex obtained is the same as the amino alcohol having one amino group, so the description is omitted.
[0083] The mixing ratio (mass ratio) of the amino alcohol relative to copper formate is preferably in the range of more than 0.6 and less than 1.5. More preferably, the mixing ratio of the amino alcohol is in the range of more than 0.6 and less than 1.0. When using more than two kinds of amino alcohols, the total amount of the amino alcohol is prepared in the above-mentioned range. Mixing can be carried out at room temperature using a stirrer, etc. When a dark blue color is visually confirmed, it can be determined that a copper complex is obtained.
[0084] Step S120: nickel formate and L 2 The amine ligand represented by L is mixed to form a nickel complex. 2 The nickel complex obtained is the same as the above-mentioned aliphatic amine having one amino group, so the description thereof is omitted.
[0085] The mixing ratio (mass ratio) of the aliphatic amine relative to nickel formate is preferably in the range of 0.75 or more and less than 2.4. More preferably, the mixing ratio of the aliphatic amine is in the range of 1.0 or more and 2.0 or less. When two or more aliphatic amines are used, the total amount of the aliphatic amines is prepared in the above range. The mixing can be performed at room temperature using a stirrer or the like. When light blue, purple, light green or dark green is visually confirmed, it can be determined that the nickel complex is obtained.
[0086] During the mixing, a polyol may be added as a solvent. This facilitates the mixing of nickel formate and aliphatic amine and promotes the formation of a nickel complex. The polyols described above may be used.
[0087] Step S130: Mix the copper complex obtained in step S110 and the nickel complex obtained in step S120. Here, the mixing is performed in such a manner that the mass ratio of the nickel complex to the copper complex satisfies 0.05 or more and less than 6. Thus, the content ratio of nickel satisfies the range of 5 mass % or more and less than 80 mass % relative to the total mass of copper and nickel in the conductive ink, and a metal wiring with less surface unevenness and no cracks can be obtained. The mixing can be performed at room temperature using a stirrer or the like.
[0088] The mixing is more preferably performed in a manner such that the mass ratio of the nickel complex to the copper complex satisfies 0.15 or more and 3.5 or less. Thus, the nickel content is in the range of 10 mass % or more and less than 70 mass % relative to the total mass of copper and nickel in the conductive ink, and a metal wiring with less surface unevenness and no cracks can be obtained.
[0089] The mixing is preferably performed in such a manner that the mass ratio of the nickel complex to the copper complex satisfies 0.3 or more and 3 or less. Thus, the content of nickel satisfies the range of 19 mass % or more and less than 67 mass % relative to the total mass of copper and nickel in the conductive ink, and a metal wiring with less surface unevenness and no cracks can be obtained.
[0090] In step S130, copper particles and / or nickel particles may be added. Thus, thick metal wiring with a thickness of several μm or more can be obtained. The addition amount or particle size of these particles is as described above, so the description is omitted. In the case of adding copper particles, the nickel content is added in a range of 5% by mass or more and less than 80% by mass relative to the total mass of copper and nickel in the final conductive ink. In the case of adding nickel particles, it is the same as the case of adding two kinds of particles.
[0091] In step S130, monohydric alcohol may be added. This adjusts the viscosity of the conductive ink and makes it an ink with excellent coating properties. The monohydric alcohol is as described above, so the description thereof is omitted.
[0092] It should be noted that although the amine ligand L in step S110 is described as 1 Using amino alcohol, as amine ligand L in step S120 2 In the case of using aliphatic amine, aliphatic amine may be used in step S110 and amino alcohol may be used in step S120. In this case as well, the above-mentioned mass ratio can be adopted.
[0093] (Implementation Method 2)
[0094] In Embodiment 2, a substrate with a copper-nickel alloy electrode and a method for producing the same according to the present invention will be described.
[0095] Figure 2 This is a schematic diagram showing a substrate with a copper-nickel alloy electrode according to the present invention.
[0096] The substrate with copper-nickel alloy electrodes (hereinafter referred to as the substrate with electrodes) 200 of the present invention comprises a substrate 210 and an electrode 220 containing a copper-nickel alloy located on the substrate 210. The electrode 220 is formed by the conductive ink described in Embodiment 1. Therefore, the content ratio of nickel satisfies the range of 5 mass % or more and 80 mass % or less relative to the total mass of copper and nickel in the copper-nickel alloy. Thus, a substrate having a smooth and crack-free electrode or metal wiring can be provided. In particular, by forming a copper-nickel alloy, it is inexpensive and has excellent atmospheric stability.
[0097] The electrode 220 may contain copper particles and / or nickel particles in addition to the copper-nickel alloy. Thus, the electrode 220 can be a thick electrode having a thickness of several μm or more. The particle size of these particles is preferably in the range of 50 nm or more and 1 μm or less, and more preferably in the range of 50 nm or more and 400 nm or less. Thus, a thick metal wiring with few surface irregularities and no cracks can be obtained.
[0098] The electrode 220 may be a surface electrode covering the entire substrate 210 , or may have a predetermined pattern such as a comb shape or a grid shape.
[0099] The substrate 210 can use a polymer substrate, Si wafer, glass, ceramic, metal plate, etc. As a polymer substrate, there is no particular limitation as long as it is resistant to temperatures around 170°C, and polyester resins represented by polyethylene naphthalate, polyimide, polyolefin resins, etc. can be preferred. The substrate is not limited to a plate shape, and can include a surface with a curvature. In addition, the substrate can be a self-supporting film. A base layer such as a semiconductor film, a metal film, a dielectric film, an organic film, etc. can be formed on the surface of the substrate. As described later, the conductive ink of the present invention can be used with a polymer substrate because it can be heated at a relatively low temperature of 170°C to form a copper-nickel alloy.
[0100] When the substrate 210 is a polymer substrate selected from the group consisting of polyethylene naphthalate, polyimide, and polyolefin resin, a flexible substrate with electrodes can be provided. Such a substrate with electrodes is advantageous for wearable devices.
[0101] Next, a method for producing a substrate with an electrode using the conductive ink for a copper-nickel alloy electrode of the present invention will be described.
[0102] Figure 3 This is a flow chart showing the steps of manufacturing the substrate with copper-nickel alloy electrodes according to the present invention.
[0103] Step S310: Apply the conductive ink for copper-nickel alloy electrode of the present invention to the substrate. The conductive ink is as described in Embodiment 1, and the description thereof is omitted. The substrate can be the above-mentioned substrate.
[0104] There are no particular restrictions on the application of the conductive ink on the substrate as long as it can form a film, and for example, a method selected from the group consisting of spin coating, spray coating, dip coating, slit coating, slot coating, rod coating, roller coating, curtain coating, gravure printing, inkjet and screen printing can be used. These methods can form a uniform film.
[0105] Step S320: The substrate coated with the conductive ink obtained in step S310 is heated (fired). As a result, copper is precipitated from the copper complex in the conductive ink, nickel is precipitated from the nickel complex, and copper reacts with nickel to form a copper-nickel alloy. In addition, amino alcohol and aliphatic amine are decomposed by heating. Here, since copper precipitation from the copper complex occurs first in the process of generating a copper-nickel alloy from the conductive ink of the present invention, the materials used in the manufacture of ink using existing copper nanoparticles listed above can be widely used as the amine ligand, i.e., amino alcohol, used in the formation of the copper complex. In addition, in the precipitation of nickel from the nickel complex, when the precipitated nickel is a dense film-like body, the reactivity with copper is improved and a fully alloyed copper-nickel alloy is easily obtained. Therefore, when the materials listed above are used as the amine ligand, i.e., aliphatic amine, used in the formation of the nickel complex, the nickel precipitated from the nickel complex is easy to become a denser film-like body, so it is preferred. It should be noted that even when a conductive ink is used in which the amine ligand used to form the copper complex is an aliphatic amine and the amine ligand used to form the nickel complex is an amino alcohol, a fully alloyed copper-nickel alloy can be obtained by appropriately selecting the types of the aliphatic amine and the amino alcohol.
[0106] The heating is preferably carried out in a temperature range of 170°C to 250°C and a time range of 1 minute to 60 minutes. In this temperature range and heating time, a copper-nickel alloy is generated. A hot plate, a thermostatic bath, an oven, etc. can be used for heating. The heating environment is preferably an inert gas environment such as nitrogen and argon. Thus, the generation of copper oxide is suppressed.
[0107] After step S320, heating (sintering) by light irradiation may be performed. Thus, the copper-nickel alloy particles are further sintered, thereby reducing the resistance. In addition, the adhesion between the electrode and the substrate can be improved. Such light irradiation can use intense pulsed light (IPL) or near-infrared laser.
[0108] Next, the present invention will be described in detail using specific examples, but please note that the present invention is not limited to these examples.
[0109] [Example]
[0110] [Reagents]
[0111] Copper formate dihydrate (HCOO) 2Cu·2H2O and nickel formate dihydrate (HCOO) 2Ni·2H2O were purchased from Fujifilm Wako Pure Chemical Industries, Ltd. Amine ligands L shown in Table 1 were purchased from Nacalai Tesque, Inc. Ethylene glycol and isopropyl alcohol were purchased from Nacalai Tesque, Inc.
[0112] [Table 1]
[0113]
[0114] Table 1: List of amine ligands L
[0115] [Example 1~Example 21]
[0116] In Examples 1 to 21, various conductive inks were prepared using copper formate dihydrate, nickel formate dihydrate, and various amine ligands L shown in Table 1, and these were used to form electrodes.
[0117] As shown in Table 2, copper formate dihydrate was mixed with 2-amino-2-methyl-1-propanol (AMP) or 2-ethylhexylamine (2EHA) to form a copper complex ( Figure 1 Step S110). The mixing was performed at room temperature (25°C) using a stirrer (manufactured by THINKY Corporation, model ARE-310). After stirring, the mixture turned dark blue as shown in Table 2, and a copper complex was formed. The obtained copper complexes were respectively called Cu-AMP and Cu-2EHA.
[0118] [Table 2]
[0119]
[0120] Table 2: List of production conditions of copper complexes
[0121] As shown in Table 3, nickel formate dihydrate and 2-amino-2-methyl-1-propanol (AMP), 2-ethylhexylamine (2EHA), ethylenediamine (ED), triethylenetetramine (TETA), hexylamine (HEA) or 2-heptylamine (2HEPA) and ethylene glycol (0.5 g) as a solvent were mixed to form a nickel complex ( Figure 1 Step S120). The mixing is performed using a stirrer at room temperature (25°C). After stirring, as shown in Table 3, it turns light blue, purple, light green or dark green, forming a nickel complex. The obtained nickel complexes are respectively called Ni-AMP, Ni-2EHA, Ni-ED, Ni-TETA, Ni-HEA and Ni-2HEPA.
[0122] [Table 3]
[0123]
[0124] Table 3: List of manufacturing conditions for nickel complexes
[0125] As shown in Table 4, the mixed copper complex and nickel complex ( Figure 1Step S130). The mixing is carried out using a stirrer at room temperature (25°C). The conductive inks of Examples 11 to 16 are the same as the conductive ink of Example 1, but the electrode formation conditions thereafter are different. In Examples 17 and 18, 1 g of copper particles (average median particle size D50: 350 nm) are added to the mixture (4.4 g) of the copper complex and the nickel complex after mixing. The conductive ink of Example 21 is not mixed with the nickel complex and is a single copper complex. The proportion of nickel content relative to the total mass of copper and nickel contained in the conductive ink obtained in this way is shown in Table 4.
[0126] [Table 4]
[0127]
[0128] Table 4: List of manufacturing conditions of conductive inks of Examples 1 to 21
[0129] *: The Ni content in the final conductive ink was 23% by mass relative to the amount of the mixture (4.4 g) of the copper complex and the nickel complex added.
[0130] The conductive inks of Examples 1 to 21 were applied by screen printing on a polyimide substrate (manufactured by Toray Industries, Inc.) and a glass substrate (manufactured by Corning). Figure 3 Step S310). It should be noted that the substrate was cleaned in an ultrasonic bath of ethanol for 15 minutes and then cleaned in distilled water for 1 minute to remove surface dirt. The substrate coated with the conductive ink was heated (sintered) under the conditions shown in Table 5 ( Figure 3 Step S320). The samples were heated in a nitrogen environment, maintained at the temperature conditions shown in Table 5 for a predetermined time, and then left to cool. In Examples 16 and 18, after heating, intense pulsed light (IPL, manufactured by NovaCentrix, PulseForge Invent) was irradiated at 400 V and 2 ms.
[0131] [Table 5]
[0132] example Firing temperature (℃) Firing time (minutes) IPL 1 230 15 - 2 230 15 - 3 230 15 - 4 230 15 - 5 230 15 - 6 230 15 - 7 230 15 - 8 230 15 - 9 230 15 - 10 230 15 - 11 250 15 - 12 210 15 - 13 210 5 - 14 190 15 - 15 170 30 - 16 230 15 400V, 2ms 17 230 15 - 18 230 15 400V, 2ms 19 230 15 - 20 230 15 - 21 230 15 -
[0133] Table 5: Firing conditions of conductive inks of Examples 1 to 21
[0134] The electrodes of Examples 1 to 21 thus obtained were evaluated. The thickness of the electrode was measured using a micro-shape measuring machine (manufactured by Kosaka Laboratory, Model ET200). The electrode surface was observed using an optical microscope (manufactured by Nikon Corporation) and a scanning electron microscope (SEM, manufactured by Hitachi High-Technologies Corporation, S-4800). Elemental mapping was performed using an energy dispersive X-ray spectrometer (EDS) attached to the SEM. These results are shown in Figures 4 to 10 .
[0135] The metals of the electrodes of Examples 1 to 21 were identified using an X-ray diffraction measuring apparatus (XRD, manufactured by Rigaku Corporation, SmartLab). The results are shown in Fig.11 The resistance of the electrodes of Examples 1 to 21 was measured by a four-terminal method (RM3545 manufactured by Hioki Electric Co., Ltd.). These results are shown in Fig.12 , Fig.13 and Table 6.
[0136] The oxidation resistance test of the electrodes of Examples 1, 6 to 8, and 21 was conducted. The test was to heat each electrode to 180°C in the atmosphere and measure the resistance after keeping it for a predetermined time. The results are shown in Fig.14 .
[0137] Figure 4 This is a diagram showing the appearance of the electrode of Example 1.
[0138] Figure 4 The upper part shows the electrodes on the glass substrate. Figure 4 The lower part of the diagram shows the electrodes on the polyimide substrate. Figure 4 The electrodes on any substrate showed metallic luster, and no bumps or cracks were found visually. Although not shown in the figure, the electrodes of Examples 6 to 9 and Examples 11 to 20 were the same. When the conductive ink of the present invention is used, since the electrodes can be formed at a relatively low temperature, a polymer substrate can also be used.
[0139] Figure 5 The figures show optical microscope photographs of the electrodes of Examples 1 to 6.
[0140] Figure 6 The figures show optical microscope photographs of the electrodes of Examples 7 to 10.
[0141] according to Figure 5 , the surface of the electrode of Example 1 is uniform, smooth and without irregularities. Although not shown in the figure, the surfaces of the electrodes of Examples 19 and 20 are also uniform, smooth and without irregularities. On the other hand, although the electrodes of Examples 2 to 5 have the same nickel content ratio as the electrode of Example 1 (the nickel content ratio relative to the total mass of copper and nickel contained in the conductive ink), they are not uniform and have irregularities, spots, cracks, etc. This shows that the conductive ink containing a copper complex composed of copper formate and a specified amino alcohol and a nickel complex composed of nickel formate and a specified aliphatic amine having one amino group is effective for obtaining a metal wiring with a smooth surface. The electrical properties of the electrode of Example 5 having cracks were not measured.
[0142] exist Figure 5 and Figure 6In the comparison of the surfaces of the electrodes of Examples 1, 6 to 10, it is shown that as the nickel content increases, there is a tendency to become uniform and smooth, but cracks occur when the nickel content is 80% by mass or more. It can be seen that when a conductive ink with a nickel content of 15% by mass or more and 70% by mass or less is used, a uniform metal wiring is obtained. This shows that it is effective for the nickel content in the conductive ink to be 5% by mass or more and less than 80% by mass.
[0143] Figure 7 This is a diagram showing a SEM image of the electrode of Example 1.
[0144] Figure 8 This is a diagram showing the EDS element distribution of the electrode of Example 1.
[0145] Fig. 9 The figures show SEM images of the electrodes of Examples 7 to 9.
[0146] Fig.10 The diagram shows SEM images of the electrodes of Examples 17 and 18.
[0147] according to Figure 7 It can be seen that the electrode of Example 1 is composed of particles having an average particle size of 75 nm or more and 150 nm or less. Figure 8 It can be seen that the particles are composed of copper (Cu) and nickel (Ni), and Cu and Ni are uniformly dispersed in the particles.
[0148] according to Fig. 9 The electrodes of Examples 7 to 9 are all composed of particles with a particle size ranging from 10 nm to 1 μm. However, compared with the particle size of the electrodes of Examples 1 and 7 to 9, it can be seen that the particle size depends on the nickel content. The smaller the nickel content, the larger the particle size, and the larger the nickel content, the smaller the particle size.
[0149] according to Fig.10 It can be seen that in the electrode of Example 18 which was irradiated with light after heating, sintering between particles was progressing compared with the electrode of Example 17.
[0150] Fig.11 It is a figure which shows the XRD spectrum of the electrode of Example 1 - Example 4.
[0151] according to Fig.11 , the electrodes of Examples 1 to 3 only show the peaks of Cu(111) and Cu(200). It can be seen that the electrodes of Examples 1 to 3 contain an alloy in which copper and nickel are uniformly mixed. Figure 8It should be noted that, although not shown, the electrodes of Examples 6 to 9 and Examples 11 to 20 also showed the same XRD spectra as the electrode of Example 1. On the other hand, the electrode of Example 4 showed peaks of Cu(111) and Cu(200) and peaks of Ni(111) and Ni(200), indicating that alloying was insufficient.
[0152] Fig.12 This is a graph showing the resistance of the electrodes of Examples 1 to 4.
[0153] Fig.13 This is a graph showing the dependence of the resistance of the electrode on the nickel content ratio.
[0154] according to Fig.12 , indicating that the electrode of Example 1 has the smallest resistance and is effective as an electrode. Fig.13 The relationship between the resistance and the nickel content of the electrodes of Examples 1, 6 to 10, and 21 is shown. Fig.13 The resistance of the electrode of Example 10 in which cracks were generated increased, but the electrodes of Examples 1, 6 to 9 in which cracks were not generated showed low resistance as well as the electrode of Example 21 which did not contain nickel. This shows that the conductive ink containing a copper complex composed of copper formate and a predetermined amino alcohol and a nickel complex composed of nickel formate and a predetermined aliphatic amine having one amino group, and containing nickel in a range of 5 mass % or more and less than 80 mass %, is effective for metal wiring.
[0155] These results are collectively shown in Table 6.
[0156] In Table 6, the meanings of the symbols in the "Formation of copper-nickel alloy" column are as follows. Circle symbol: an alloy in which copper and nickel are uniformly mixed is generated; Triangle symbol: copper and nickel are not sufficiently alloyed; Cross symbol: no nickel complex is used in the manufacture of the conductive ink. In addition, the "Morphology" column briefly shows the state of the surface of each of the above electrodes.
[0157] [Table 6]
[0158] example Formation of copper-nickel alloy Electrode thickness (μm) form Resistance(Ω) 1 ○ 1.5 Very smooth 25 2 ○ 1.5 Concave and convex 4000 3 ○ 1.5 Concave and convex 175 4 △ 1.5 Concave and convex 200 5 ○ 1.5 Many cracks - 6 ○ 1.5 There are bumps 5.7 7 ○ 1.5 smooth 9.5 8 ○ 1.5 There are bumps 27 9 ○ 1.5 Very smooth 35 10 ○ 1.5 There are cracks 160 11 ○ 1.5 smooth 26 12 ○ 1.5 smooth 28 13 ○ 1.5 smooth 30 14 ○ 1.5 smooth 48 15 ○ 1.5 smooth 29 16 ○ 1.5 smooth 7 17 ○ 3 smooth 4 18 ○ 3 smooth 2 19 ○ 1.5 smooth 38 20 ○ 1.5 smooth 65 21 × 3 There are bumps 5
[0159] Table 6: Characteristics of electrodes obtained from conductive inks of Examples 1 to 21
[0160] According to Table 6, it is shown that when a conductive ink containing a copper complex composed of copper formate and a specified amino alcohol and a nickel complex composed of nickel formate and a specified aliphatic amine having one amino group is used, and the nickel content is in the range of 5 mass % or more and less than 80 mass %, smooth metal wiring without bumps and depressions can be provided.
[0161] Fig.14 It is a graph showing the results of the oxidation resistance test.
[0162] according to Fig.14 The electrodes of Examples 1, 6 to 8 obtained from the conductive ink of the present invention maintained low resistance even after being heated in the atmosphere, but the electrode of Example 21 which did not contain nickel had an increased resistance as the heating time in the atmosphere increased, and lost its function as an electrode. This is because the electrodes of Examples 1, 6 to 8 are made of copper-nickel alloy, and therefore copper oxide is not generated even when heated in the atmosphere. This shows that the conductive ink of the present invention is advantageous for generating an electrode made of a copper-nickel alloy having excellent oxidation resistance.
[0163] Industrial Applicability
[0164] When the conductive ink of the present invention is used, a metal wiring having excellent atmospheric stability and a smooth surface can be provided at a low price using an inexpensive material.
[0165] Description of Reference Numerals
[0166] 200: Substrate with copper-nickel alloy electrodes.
[0167] 210: Substrate.
[0168] 220: Electrode containing copper-nickel alloy.
Claims
1. A conductive ink, which is a conductive ink for copper-nickel alloy electrodes, wherein: The conductive ink contains a copper complex represented by general formula A and a nickel complex represented by general formula B. The content ratio of nickel is in the range of 10 mass % or more and 70 mass % or less relative to the total mass of copper and nickel. Cu(HCOO)2(L 1 ) m A Ni(HCOO)2(L 2 ) n B Here, m and n are natural numbers from 2 to 6, respectively, and L 1 is 2-amino-2-methyl-1-propanol, L 2 It is 2-ethylhexylamine, or the opposite.
2. The conductive ink according to claim 1, wherein: The nickel content is in the range of 19 mass % or more and 67 mass % or less.
3. The conductive ink according to claim 2, wherein: The nickel content is in the range of 23 mass % or more and 67 mass % or less.
4. The conductive ink according to claim 3, wherein: The nickel content is in the range of 30 mass % or more and 50 mass % or less.
5. The conductive ink according to any one of claims 1 to 4, wherein The conductive ink further contains copper particles and / or nickel particles.
6. The conductive ink according to any one of claims 1 to 4, wherein The conductive ink further contains copper particles or copper particles and nickel particles.
7. The conductive ink according to any one of claims 1 to 4, wherein The conductive ink further contains a monohydric alcohol and / or a polyhydric alcohol.
8. The conductive ink according to claim 7, wherein: The monohydric alcohol is selected from the group consisting of methanol, ethanol, 1-propanol, 1-butanol, 2-butanol, 2-methyl-1-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 3-methyl-1-butanol, 2-methyl-1-butanol, 2,2-dimethyl-1-propanol, 3-methyl-2-butanol and 2-methyl-2-butanol.
9. The conductive ink according to claim 7, wherein: The polyol is selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, butylene glycol, pentylene glycol, dipropylene glycol, tripropylene glycol, polyethylene glycol, polypropylene glycol and glycerol.
10. A method for manufacturing a conductive ink for copper-nickel alloy electrodes, wherein: The method comprises: Copper formate and L 1 The amine ligands represented are mixed to form a copper complex; Nickel formate and L 2 Mixing the amine ligand represented by to form a nickel complex; and The copper complex and the nickel complex are mixed so that the mass ratio of the nickel complex to the copper complex satisfies 0.15 or more and 3.5 or less, The L 1 is 2-amino-2-methyl-1-propanol, said L 2 It is 2-ethylhexylamine, or the opposite.
11. The method of claim 10, wherein: In the mixing, the copper complex and the nickel complex are mixed so that a mass ratio of the nickel complex to the copper complex satisfies 0.3 or more and 3 or less.
12. The method according to claim 10 or 11, wherein: In the formation of the nickel complex, a polyol is further mixed.
13. The method of claim 12, wherein: The polyol is selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, butylene glycol, pentylene glycol, dipropylene glycol, tripropylene glycol, polyethylene glycol, polypropylene glycol and glycerol.
14. The method according to claim 10 or 11, wherein: During the mixing, a monohydric alcohol is further added.
15. The method according to claim 10 or 11, wherein: During the mixing, copper particles and / or nickel particles are further mixed.
16. The method according to claim 10 or 11, wherein: In the mixing, copper particles are further mixed or copper particles and nickel particles are further mixed.
17. A substrate with a copper-nickel alloy electrode, wherein: The substrate with copper-nickel alloy electrodes comprises: substrate; and an electrode comprising a copper-nickel alloy disposed on the substrate, The content ratio of nickel in the copper-nickel alloy relative to the total mass of copper and nickel is in a range of 10 mass % to 70 mass %.
18. The substrate according to claim 17, wherein The content ratio of nickel in the copper-nickel alloy relative to the total mass of copper and nickel is in a range of 19 mass % to 67 mass %.
19. The substrate according to claim 17 or 18, wherein The substrate is selected from the group consisting of polyethylene naphthalate, polyimide and polyolefin resin.
20. The substrate according to claim 17 or 18, wherein The electrode further contains copper particles and / or nickel particles.
21. The substrate according to claim 17 or 18, wherein The electrode further contains copper particles or copper particles and nickel particles.
22. A method of manufacturing a substrate with a copper-nickel alloy electrode, wherein: The method comprises: applying the conductive ink according to any one of claims 1 to 9 to a substrate; and The substrate coated with the conductive ink is heated.
23. The method of claim 22, wherein: The coating is performed using a method selected from the group consisting of spin coating, spray coating, dip coating, slit coating, slot coating, rod coating, roll coating, curtain coating, gravure printing, inkjet and screen printing.
24. The method of claim 22 or 23, wherein: The heating is performed at a temperature range of 170° C. to 250° C. and for a time range of 1 minute to 60 minutes.