Polymer fiber membrane containing carbon layer structure and preparation method thereof

The preparation of polymer composite fiber membranes with high specific surface area through near-infrared laser irradiation technology solves the problems of high energy consumption and difficulty in recycling during the preparation of porous adsorbent materials, and realizes the application of efficient and environmentally friendly carbon adsorbent materials in the field of water treatment.

CN116356601BActive Publication Date: 2024-12-03JIANGSU ZHUOYUE INTELLIGENT ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310197599.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-03
Publication Date
2024-12-03
Estimated Expiration
2043-03-03

AI Technical Summary

Technical Problem

During the preparation process, existing porous adsorbent materials have problems such as high energy consumption, complex process, polluting the environment and not easy to recycle and use in powder or block forms, and it is difficult to effectively apply to the water treatment field.

Method used

Using in-situ carbonization technology of polymer materials under near-infrared laser radiation, a polymer composite fiber membrane with high specific surface area and easy recovery is prepared, forming a new type of carbon adsorption with laser carbonized structure as the surface layer and polymer fiber structure as the support layer. Materials, carbonized structures of varying degrees are constructed by adjusting the composite fiber ratio and laser parameters.

Benefits of technology

It realizes low-cost, simple process and efficient preparation of carbon adsorbent materials, avoids the easy shedding of carbon powder and environmental pollution, is suitable for water treatment, and can carry out large-scale and efficient carbonization of polymer composite fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004107737110000011
    Figure HDA0004107737110000011
  • Figure HDA0004107737110000012
    Figure HDA0004107737110000012
  • Figure HDA0004107737110000021
    Figure HDA0004107737110000021
Patent Text Reader

Abstract

The present invention belongs to the field of polymer materials, and specifically relates to a polymer fiber membrane containing a carbon layer structure and a preparation method thereof. The polymer composite fiber is sheared and shredded by a blender, and then filtered to form a dense fiber membrane. Subsequently, under the induction of laser irradiation, the surface of the fiber membrane absorbs a large amount of laser energy to undergo a carbonization reaction to form a carbon layer. During the laser irradiation process of the fiber membrane: the laser first acts on the surface of the polymer composite fiber, and the polymer resin that easily absorbs laser energy absorbs a large amount of laser energy, undergoes a carbonization reaction, and forms a carbonized structure; the excess laser energy is transmitted to the resin that is not easy to absorb laser energy, causing it to melt, and the porous carbon material formed by carbonization adheres to the surface of the molten resin fiber to form a carbonized layer of a certain thickness. A large number of carbon particles in the carbonized layer have a mesoporous structure, which can adsorb small molecular dyes in water and have a high adsorption capacity for organic dyes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials, and in particular relates to a polymer fiber membrane containing a carbon layer structure and a preparation method thereof. Background Art

[0002] Organic dyes are a major pollutant in industrial wastewater and domestic sewage, and have always been a major problem plaguing society. Currently, porous adsorption materials are usually used to adsorb and filter dyes in wastewater. Commonly used adsorption materials include activated carbon, porous zeolite, porous alumina, etc. These porous materials usually have the following problems in practical applications:

[0003] (1) The preparation process relies on high temperature, which generally results in high energy consumption, many steps, and a long time.

[0004] (2) The pore structure control processes such as template method and activation method are complex, have low applicability, and pollute the environment during the process;

[0005] (3) Porous adsorption materials mostly exist in the form of powder or block, which limits their practical application scenarios and makes them difficult to recycle.

[0006] Therefore, exploring a simpler and more efficient carbon adsorption material and its preparation method is an urgent need for further promotion and application of adsorption materials.

[0007] Laser technology was born in the 1960s and is widely used in the processing field. Its principle is that the laser emits a high-energy laser beam to scan the surface of the processing material, so that a certain physical reaction or carbonization chemical reaction occurs on the surface of the processing material. Compared with the traditional high-temperature carbonization method, the near-infrared (1064nm) laser in-situ carbonization technology only needs to be implemented at room temperature, and has the characteristics of low energy consumption, high efficiency, and environmental friendliness. However, since the carbonized structure of polymers under laser irradiation is a powder, it cannot be directly applied to fields such as water treatment. There are problems such as difficulty in recycling and secondary pollution. Therefore, laser in-situ carbonization is currently mostly used for pattern marking on the surface of polymer materials. Summary of the invention

[0008] The present invention provides a polymer fiber membrane containing a carbon layer structure and a preparation method thereof. Based on the in-situ carbonization mechanism of polymer materials under near-infrared laser irradiation, a polymer composite fiber membrane with a high specific surface area and easy to recycle is prepared, and near-infrared laser controllable carbonization is performed on its surface. Finally, a new type of carbon adsorption material with a laser carbonization structure as the surface layer and a polymer fiber structure as the supporting layer is prepared. While efficiently preparing the carbon adsorption material, its carbonization structure can be precisely controlled.

[0009] The method for preparing the polymer fiber membrane containing a carbon layer structure provided by the present invention has the characteristics of low cost, simple process, high adsorption and filtration efficiency, and is prepared by the following steps:

[0010] (1) Two or more polymer fibers are mixed in an ethanol solution in proportion, and a stirrer is used to shear at a speed of 300-1000 rpm for 2-10 minutes at room temperature to prepare a suspension. The suspension is poured into a Buchner funnel for suction filtration to obtain a membrane-like composite fiber, and the fiber membrane is placed in a vacuum oven at 60° C. for 10 hours to completely evaporate the ethanol, thereby preparing a film having a thickness of 0.1-3 cm and a density of 0.8-0.9 g / cm 3 , area 0.1-2m 2 The polymer composite fiber membrane is ready for use.

[0011] Polymer fibers refer to all polymers that have different absorption of 1064nm wavelength laser, including but not limited to aramid fibers, polypropylene, polyacrylonitrile, polystyrene, polycarbonate and other polymer systems that can be prepared into fibers.

[0012] Preferably, the polymer fibers are composed of polymer fibers that easily absorb laser energy and polymer fibers that do not easily absorb laser energy.

[0013] Among them, polymer fibers that easily absorb laser energy include aramid fibers, polystyrene fibers, polycarbonate fibers, and the like.

[0014] The polymer fibers that are not easy to absorb laser energy are polypropylene fibers, polyethylene fibers, polyacrylonitrile fibers, etc.

[0015] The mass ratio of the polymer fiber that easily absorbs laser energy to the polymer fiber that does not easily absorb laser energy is 10:90-50:50.

[0016] (2) The prepared polymer composite fiber membrane is treated with near-infrared laser irradiation, and the laser current is adjusted to 5-15A, the spot size is 1-10μm, and the scanning rate is 100-2000mm / s. Under this condition, different polymer fibers undergo laser-induced carbonization reactions to varying degrees, thereby forming carbonized layers with different pore structures on the surface, and finally preparing a double-layer structure polymer fiber membrane with a carbonized layer on the surface and a fiber filtration layer on the bottom layer.

[0017] In the present invention, the carbonized layer is composed of polymer fibers with different laser responsiveness. Due to the difference in absorbing laser energy, different degrees of melting, thermal degradation and carbonization occur, and finally a dense carbonized layer structure is formed.

[0018] The laser is a yttrium aluminum garnet crystal pulse laser, the laser current is set to 5-15A, and the pulse laser wavelength is: 1064nm.

[0019] The prepared polymer fiber membrane is used for adsorption of small molecular organic dyes in water.

[0020] The principle of the present invention is:

[0021] (1) In the first step, the laser first acts on the polymer fiber that easily absorbs laser energy, causing carbonization to occur and generate a porous carbonized structure;

[0022] (2) In the second step, the excess laser energy is then transferred to the polymer fiber that does not easily absorb laser energy, causing it to melt, so that the carbonized material generated in the first step is adhered to the fiber surface, thereby forming a carbonized layer structure.

[0023] The polymer fiber membrane containing a carbon layer structure prepared by the present invention has a simple process, and the prepared polymer membrane can be directly applied to the field of water treatment, has little effect on the mechanical strength of the membrane, and can realize large-scale and efficient carbonization treatment of polymer composite fibers (schematic diagram as shown in the figure) Figure 1 It has broad application prospects in the field of water treatment.

[0024] Compared with other traditional carbon adsorption materials, the present invention avoids the phenomenon of carbon powder falling off easily during water treatment of carbon material adsorbents, and does not cause environmental pollution. Compared with traditional fiber adsorption materials, it does not require complex spinning and pore-forming processes, and there is no pollution during the preparation process. The present invention can realize large-scale and efficient preparation of polymer fiber adsorption materials with carbon layer structures. By changing the composite fiber ratio and laser parameters, different degrees of carbonization structures can be constructed on the surface of the polymer fiber membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic diagram of the preparation principle of a polymer fiber membrane containing a carbon filter layer.

[0026] Figure 2 These are scanning electron microscope and transmission electron microscope photographs of the fiber after laser irradiation in Example 1.

[0027] Figure 3 This is a side scanning electron microscope photograph of the carbonized layer of the composite fiber membrane after laser irradiation in Example 1.

[0028] Figure 4 This is the pore size distribution curve of the composite fiber membrane after laser irradiation in Example 1.

[0029] Figure 5 These are the X-ray photoelectron spectra of the composite fiber membrane of Example 2 before (a) and after (b) laser irradiation.

[0030] Figure 6 These are scanning electron microscope photos of composite fiber membranes with different ratios after laser irradiation.

[0031] Figure 7are scanning electron microscope photos of composite fiber membranes obtained under different irradiation conditions.

[0032] Figure 8 This is a scanning electron microscope photo of a single polypropylene fiber membrane after laser irradiation.

[0033] Fig. 9 This is a scanning electron microscope photo of a single polystyrene fiber membrane after laser irradiation. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further explained below in conjunction with specific implementation schemes, but it is not intended to limit the protection scope of the present invention.

[0035] Example 1

[0036] like Figure 1 Shown is a schematic diagram of the preparation principle of a polymer fiber membrane containing a carbon filter layer.

[0037] 50 parts of short aramid fiber and 100 parts of polypropylene fiber were placed in 500 parts of ethanol and the fibers were minced with a mixer at room temperature (25°C) at a speed of 300 r / min for 5 minutes. After stirring, the suspension was filtered and dried in a vacuum oven at 60°C to obtain a polymer composite fiber membrane (thickness 0.2 cm, density 0.85 g / cm 3 , area 0.3m 2 ).

[0038] The composite fiber membrane was treated with laser irradiation (laser current was 11A, spot size was 8μm, scanning rate was 1300mm / s), and "villi-like" carbon material was generated in situ on the composite fiber membrane. The scanning electron micrograph of the morphology of the fiber after carbonization is shown in FIG. Figure 2 (a) (where a2 is a partial enlarged photo of a1), the transmission electron microscope image of the generated carbon material is as follows: Figure 2 (b) (where b2 is a partial enlarged photo of b1). The side scanning electron microscope photo of the carbonized layer of the composite fiber membrane after laser irradiation is shown in Figure 3 (a, b, c, d are photos of the same part at different magnifications). The fiber membrane after laser irradiation was characterized by BET specific surface area test, and the obtained BET curve is shown in Figure 4 As shown. The specific surface area of ​​the fiber membrane is 419m 2 / g. Due to the different absorption degrees of laser by different polymer fibers, the pore size formed by carbonized polymer fibers is smaller, while the pore size formed by melted polymer fibers is larger. The overall pore size distribution is 10 1 -10 55g of the composite fiber membrane was immersed in 200ml of a 200mg / L methylene blue solution, and the adsorption efficiency in five minutes (the methylene blue concentration was calculated by ultraviolet absorption spectrum, adsorption efficiency = (initial methylene blue concentration - remaining methylene blue concentration) / initial methylene blue concentration) was 98.3%.

[0039] Example 2

[0040] 120 parts of polyacrylonitrile fiber and 110 parts of polycarbonate fiber were placed in 700 parts of ethanol and the fibers were minced with a mixer at room temperature (25°C) at a speed of 400 r / min for 11 minutes. After stirring, the suspension was filtered and dried in a vacuum oven at 60°C to obtain a polymer composite fiber membrane (thickness 0.3 cm, density 0.92 g / cm 3 , area 0.4m 2 The composite fiber membrane was subjected to laser irradiation treatment (laser current was 10A, spot size was 10μm, and scanning rate was 1200mm / s). Figure 5 As shown, the carbon content of the fiber membrane surface before and after laser irradiation was characterized by X-ray photoelectron spectroscopy. The carbon content of the fiber membrane surface increased from 92.59% to 96.81%, which was caused by the formation of the carbonized layer. 7g of the composite fiber membrane was immersed in 300ml of a 100mg / L methylene blue solution, and the adsorption efficiency was 97.8% in five minutes.

[0041] Example 3

[0042] 50 parts of polystyrene fiber and 250 parts of polypropylene fiber were placed in 1000 parts of ethanol, and the fibers were minced with a mixer at room temperature (25°C) at a speed of 400r / min for 11 minutes. After stirring, the suspension was filtered and dried in a vacuum oven at 60°C to obtain a polymer composite fiber membrane (thickness 0.3cm, density 0.89g / cm 3 , area 0.25m 2 The composite fiber membrane was treated with laser irradiation (laser current was 7A, spot size was 9μm, scanning rate was 500mm / s), and the scanning electron micrograph of the fiber carbonization morphology was shown in Figure 6 As shown in (a) (where a2 is a partial enlarged photo of a1), due to the low content of polystyrene, no obvious carbonized structure is observed on the fiber surface, and only some large holes exist. 7g of the composite fiber membrane was immersed in 300ml of a 100mg / L methylene blue solution, and the adsorption efficiency was 40.1% in five minutes.

[0043] Example 4

[0044] 100 parts of polystyrene fiber and 200 parts of polypropylene fiber were placed in 1000 parts of ethanol, and the fibers were minced with a mixer at room temperature (25°C) at a speed of 400r / min for 11 minutes. After stirring, the suspension was filtered and dried in a vacuum oven at 60°C to obtain a polymer composite fiber membrane (thickness 0.3cm, density 0.89g / cm 3 , area 0.25m 2 The composite fiber membrane was treated with laser irradiation (laser current was 7A, spot size was 9μm, scanning rate was 500mm / s), and the scanning electron micrograph of the fiber carbonization morphology was shown in Figure 6 As shown in (b) (b2 is a partial enlarged photo of b1), due to the increase in the content of polystyrene, an obvious fuzzy carbonized structure is observed on the fiber surface. 7g of the composite fiber membrane was immersed in 300ml of a 100mg / L methylene blue solution, and the adsorption efficiency was 94.1% in five minutes.

[0045] Example 5

[0046] 200 parts of polystyrene fibers and 100 parts of polypropylene fibers were placed in 1000 parts of ethanol, and the fibers were minced with a mixer at room temperature (25°C) at a speed of 400 r / min for 11 minutes. After stirring, the suspension was filtered and dried in a vacuum oven at 60°C to obtain a polymer composite fiber membrane (thickness 0.3 cm, density 0.89 g / cm 3 , area 0.25m 2 The composite fiber membrane was treated with laser irradiation (laser current was 7A, spot size was 9μm, scanning rate was 500mm / s), and the scanning electron micrograph of the fiber carbonization morphology was shown in Figure 6 As shown in (c) (c2 is a partial enlarged photo of c1), due to the further increase in the content of polystyrene, the excessive laser energy absorbed causes the fiber surface to break down and adhere, and the resulting carbonized structure is wrapped by the fiber. 7g of the composite fiber membrane was immersed in 300ml of a 100mg / L methylene blue solution, and the adsorption efficiency was 81.6% in five minutes.

[0047] Example 6

[0048] 100 parts of polystyrene fiber and 200 parts of polypropylene fiber were placed in 1000 parts of ethanol, and the fibers were minced with a mixer at room temperature (25°C) at a speed of 400r / min for 11 minutes. After stirring, the suspension was filtered and dried in a vacuum oven at 60°C to obtain a polymer composite fiber membrane (thickness 0.3cm, density 0.89g / cm 3 , area 0.25m 2The composite fiber membrane was treated with laser irradiation (laser current was 4A, spot size was 10μm, scanning rate was 1000mm / s), and the scanning electron micrograph of the fiber carbonization morphology was as follows: Figure 7 As shown in the figure, due to the change of laser parameters, the composite fiber membrane under this ratio absorbs insufficient laser energy, and only adhesion is observed on the fiber surface, without obvious carbonization structure. 7g of composite fiber membrane was immersed in 300ml of methylene blue solution with a concentration of 100mg / L, and the adsorption efficiency was 51.3% in five minutes.

[0049] Comparative Example 1

[0050] Take 300 parts of polypropylene fibers, place them in 1000 parts of ethanol, and mince the fibers with a mixer at room temperature (25°C), with a rotation speed of 600r / min and a stirring time of 7 minutes. After stirring, the suspension is filtered and dried in a vacuum oven at 60°C to obtain a polypropylene fiber membrane, which is then irradiated with laser (laser current is 7A, spot size is 9μm, and scanning rate is 500mm / s). The surface morphology of the final polypropylene fiber membrane is shown in the scanning electron microscope. Figure 8 As shown in the figure, no obvious carbonized structure can be observed, and since polypropylene fibers do not easily absorb laser energy, only a large area of ​​melt adhesion is formed.

[0051] Comparative Example 2

[0052] Take 300 parts of polystyrene fibers, place them in 1000 parts of ethanol, and mince the fibers with a mixer at room temperature (25°C), with a rotation speed of 600r / min and a stirring time of 7 minutes. After stirring, the suspension is filtered and dried in a vacuum oven at 60°C to obtain a polystyrene fiber membrane, which is then irradiated with laser (laser current is 7A, spot size is 9μm, and scanning rate is 500mm / s). The surface morphology of the polystyrene fiber membrane obtained is shown in the scanning electron microscope. Fig. 9 As shown, due to the absorption of excessive laser energy, the polystyrene fiber membrane is severely carbonized, and no obvious fiber morphology can be observed. Only irregular carbonized areas can be observed. Such fiber membranes cannot be used in the field of water treatment due to clogged pores.

[0053] The above embodiments are only used to illustrate the technical solution of the present invention, and the description is more specific and detailed, rather than limiting it. For those skilled in the art, various changes and variations can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. An application of a polymer fiber membrane containing a carbon layer structure, characterized in that: The polymer fiber membrane is used for the adsorption of small molecular organic dyes in water; the polymer fiber membrane has a double-layer structure, wherein the surface layer is a carbonized layer and the bottom layer is a fiber filtration layer; the specific steps of the preparation method of the polymer fiber membrane containing the carbon layer structure are as follows: (1) Two or more polymer fibers are mixed in ethanol in a certain proportion, and the polymer system suspension is prepared by shearing and crushing with a blender at room temperature. The suspension is poured into a Buchner funnel for suction filtration to obtain a membrane fiber, and the fiber membrane is placed in a vacuum oven at 60°C to completely evaporate the ethanol, thereby obtaining a polymer composite fiber membrane for use; The polymer fibers are composed of polymer fibers that easily absorb laser energy and polymer fibers that do not easily absorb laser energy; The mass ratio of the polymer fiber that easily absorbs laser energy to the polymer fiber that does not easily absorb laser energy is 10:90-50:50; Among them, the polymer fibers that easily absorb laser energy are aramid fibers, polystyrene fibers, and polycarbonate fibers; The polymer fibers that are not easy to absorb laser energy are polypropylene fibers, polyethylene fibers, and polyacrylonitrile fibers; (2) Using a fiber laser marking machine to irradiate the prepared polymer composite fiber membrane with laser, adjusting the laser current, spot size, and scanning rate to prepare a polymer membrane; The laser current is 5-15 A, the spot size is 1-10 μm, and the scanning rate is 100-2000 mm / s; The laser is a yttrium aluminum garnet crystal pulse laser, and the pulse laser wavelength is: 1064 nm.

2. The use of the polymer fiber membrane containing a carbon layer structure as claimed in claim 1, characterized in that: The thickness of the polymer composite fiber membrane in step (1) is 0.1-3 cm, and the density is 0.8-0.9 g / cm 3 , area 0.1-2 m 2 .