A spinel thermistor material for high temperature and wide temperature range temperature measurement and its preparation method
Patent Information
- Application Number
- CN202310589422.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-24
AI Technical Summary
但是,这些方法并不能明显降低材料热敏常数(B值),并且增加了制备难度
[0017] 1)Mg x Mn 1-x Al 2x Fe 2(1-x) O 4 Extending the temperature measurement range of spinel-type thermosensitive ceramics to the high-temperature zone enables temperature measurement in high-temperature and wide-temperature zones;
Smart Images

Figure CN116621573B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a spinel thermistor material for high-temperature and wide-temperature-range temperature measurement and a preparation method thereof. The thermistor material has an obvious negative temperature coefficient characteristic in the temperature range of 0-600°C, and the linear fitting Pearson's r coefficients of lnρ and 1000 / T are both greater than or equal to 99.76%. The thermistor material is suitable for manufacturing high-temperature and wide-temperature-range thermistors. Background Art
[0002] Negative temperature coefficient thermistor ceramic materials have unique advantages over traditional temperature sensors in terms of high precision, fast response, low cost and small size, making them an ideal material for accurate temperature measurement. The general structural formula of spinel thermistor materials is AB2O4. Traditional spinel structures such as Li-Mn-O, Ni-Mn-O, Mn-Co-Ni-O, etc. are usually used under low temperature conditions. Since spinel NTC thermistor ceramic materials have the advantages of relatively mature technology, wide application and good compatibility with devices, researchers mainly conduct research on new spinel NTC thermistors through doping modification, hoping that spinel materials can be used in high temperature fields.
[0003] Magnesium aluminum spinel (MgAl2O4) has the characteristics of high temperature stability and wide band gap. It is widely used in refractories, catalysts and humidity sensors in various industries. The elements in the AB position of the magnesium aluminum spinel structure are easily replaced, so its advantage is that completely different properties can be obtained by replacing different elements. Although the production process of spinel thermistor ceramics is mature, its development is still limited due to its own defects. There are currently two main problems. Single-component magnesium aluminum spinel is an insulator with poor conductivity. Even at high temperatures, the resistivity of magnesium aluminum spinel is 10 6 Ω.cm or more. Due to the poor sintering activity of the powder, the sintering temperature of the ceramic is very high, usually at 1600℃ and above. In order to solve the above two problems, researchers have mainly studied the new spinel NTC thermistor through doping modification and composite modification methods, usually doping variable valence elements at the B position of the spinel. However, these methods cannot significantly reduce the thermal constant (B value) of the material and increase the difficulty of preparation. Therefore, it is necessary to adopt a new material modification method.
[0004] The structure of spinel manganese ferrite (MnFe2O4) is usually an inverse spinel or semi-inverse spinel structure. Like MgAl2O4, it belongs to the Fd-3m space group and can form a stable solid solution with it. Because it contains two variable valence elements, Mn and Fe, it has good conductivity. At the same time, the sintering temperature of spinel manganese ferrite is also low, which can reduce the difficulty of preparation to a certain extent.
[0005] Based on the characteristics of two solid solution units, the present invention synthesizes MgO which can be used in the range of 0-600℃. x Mn 1- x Al 2x Fe 2(1-x) O4 spinel high temperature thermistor material. Tests have shown that it has good negative temperature coefficient thermistor properties, and the content of variable valence ions can be adjusted by configuring different solid solution ratios, which can directly affect the high temperature stability and electrical transport properties of the ceramic. The solid solution material obtained by solid solution modification has the characteristics of two solid solution units, MgAl2O4 and MnFe2O4, namely high temperature stability and reduced resistance value, so the chemical formula is Mg x Mn 1-x Al 2x Fe 2(1-x) O4-based spinel ceramics are suitable as thermosensitive materials due to their high temperature stability and multivalent states of variable valence elements. Summary of the invention
[0006] The object of the present invention is to provide a spinel thermistor material for high temperature and wide temperature range temperature measurement and a preparation method thereof. The thermistor material is made of magnesium oxide, aluminum oxide, manganese dioxide and iron oxide as raw materials, and is subjected to mixed grinding, pre-sintering, cold isostatic pressing, high temperature sintering, electrode coating and other steps to obtain a thermistor material with a chemical composition of Mg x Mn 1-x Al 2x Fe 2(1-x) O4, where 0.2≤x≤0.8, the crystal structure is spinel structure, and the material constant is B 150℃ / 500℃ =4383K-7609K, the resistivity is between 2.6×10 7 Ω.cm-2.25×10 3 The linear fitting Pearson's r coefficients of Ω.cm, lnρ and 1000 / T are all greater than or equal to 99.76%, and it is a spinel thermistor material suitable for manufacturing high-temperature and wide-temperature-range thermistors.
[0007] The spinel thermistor material for high temperature and wide temperature range temperature measurement of the present invention is made of magnesium oxide, aluminum oxide, manganese dioxide and iron oxide as raw materials, and the chemical composition is Mg x Mn 1-x Al 2x Fe 2(1-x) O4, where 0.2≤x≤0.8, the crystal structure of the resistor material is a spinel structure, and the specific operation is carried out in the following steps:
[0008] a. Press Mg x Mn 1-x Al2x Fe 2(1-x) O4, 0.2≤x≤0.8 molar ratio, weigh the raw materials magnesium oxide, aluminum oxide, manganese dioxide and iron oxide respectively, put them in an agate mortar and grind them for 8-10 hours, then calcine them at a temperature of 1100-1200℃ for 2-3 hours, and grind them again for 6-8 hours to obtain single-phase Mg x Mn 1-x Al 2x Fe 2(1-x) O4 powder;
[0009] b. The powder material obtained in step a is heated to 10-25 kg / cm 2 The briquetting process is carried out under a pressure of 10-30 seconds, and the formed green body is subjected to cold isostatic pressing, maintained at a pressure of 200-350 MPa for 2-5 minutes, and then sintered at a temperature of 1300-1400°C for 0.5-6 hours to obtain Mg x Mn 1-x Al 2x Fe 2(1-x) O4 disc-shaped high-density ceramic block material;
[0010] c. Coat the front and back sides of the disc-shaped high-density ceramic block material sintered in step b with platinum slurry electrodes, and then keep it at 900°C for 30 minutes to obtain a temperature range of 0-600°C and a material constant of B. 150℃ / 500℃ =4383K-7609K, the resistivity is between 2.60×10 7 Ω.cm-2.25×10 3 The linear fitting Pearson's r coefficients of Ω.cm, lnρ and 1000 / T are all greater than or equal to 99.76% of high-temperature and wide-temperature range spinel thermistor materials.
[0011] A method for preparing a spinel thermistor material for high-temperature and wide-temperature range temperature measurement is carried out according to the following steps:
[0012] a. Press Mg x Mn 1-x Al 2x Fe 2(1-x) O4, 0.2≤x≤0.8 molar ratio, weigh the raw materials magnesium oxide, aluminum oxide, manganese dioxide and iron oxide respectively, put them in an agate mortar and grind them for 8-10 hours, then calcine them at a temperature of 1100-1200℃ for 2-3 hours, and grind them again for 6-8 hours to obtain single-phase Mg x Mn 1-x Al 2x Fe 2(1-x) O4 powder;
[0013] b. The powder material obtained in step a is heated to 10-25 kg / cm 2 The briquetting process is carried out under a pressure of 10-30 seconds, and the formed green body is subjected to cold isostatic pressing, and the pressure is maintained at 200-350 MPa for 2-5 minutes, and then sintered at a temperature of 1300℃-1400℃ for 0.5-6 hours to obtain Mg x Mn 1-x Al 2x Fe 2(1-x) O4 disc-shaped high-density ceramic block material;
[0014] c. Coat the front and back sides of the disc-shaped high-density ceramic block material sintered in step b with platinum slurry electrodes, and then keep it at 900°C for 30 minutes to obtain a temperature range of 0-600°C and a material constant of B. 150℃ / 500℃ =4383K-7609K, the resistivity is between 2.60×10 7 Ω.cm-2.25×10 3 The linear fitting Pearson's r coefficients of Ω.cm, lnρ and 1000 / T are all greater than or equal to 99.76% of high-temperature and wide-temperature range spinel thermistor materials.
[0015] The present invention discloses a spinel thermistor material for high temperature and wide temperature range temperature measurement. The thermistor material is made of magnesium oxide, aluminum oxide, manganese dioxide and iron oxide as raw materials, and is obtained by mixed grinding, calcination, cold isostatic pressing, high temperature sintering and electrode coating. The method realizes the preparation of a single spinel high temperature thermistor under normal pressure. The process has low requirements on equipment, simple operation process and can realize mass production. The chemical composition system is Mg x Mn 1-x Al 2x Fe 2(1-x) O4, where 0.2≤x≤0.8. By adjusting the solid solution ratio to adjust the electrical properties of the system thermistor material, a high-temperature and wide-temperature range thermistor with adjustable electrical properties is manufactured.
[0016] Beneficial effects: Compared with the prior art, the present invention has the following advantages:
[0017] 1) Mg x Mn 1-x Al 2x Fe 2(1-x) O4 increases the temperature measurement range of spinel thermistor ceramics to high temperature range, and can achieve temperature measurement in high temperature and wide temperature range;
[0018] 2) The present invention realizes the preparation of a single spinel high-temperature thermistor under normal pressure. This process has low equipment requirements, a simple operation process, and can achieve mass production;
[0019] 3) The material constant of the thermistor is B 150℃ / 500℃ =4383K-7609K, and this range can be adjusted by changing the solid solution ratio. The resistivity of the material is 2.6×10 7 Ω.cm-2.25×10 3 The linear fitting Pearson's r coefficients of Ω.cm, lnρ and 1000 / T are all greater than or equal to 99.76%. The resistance drift rate is less than 2.24% after aging at 1000℃ for 1000 hours. It has the advantages of stable performance, high accuracy, high sensitivity and good consistency. The specific performance parameters are shown in Table 1.
[0020] Table 1
[0021] BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is the X-ray diffraction pattern of the thermistor material of the present invention (without platinum paste electrode coating).
[0023] Figure 2 It is the resistance-temperature characteristic curve of the thermistor ceramic of the present invention. DETAILED DESCRIPTION
[0024] Example 1 (x=0.8)
[0025] a. Press Mg 0.8 Mn 0.2 Al 1.6 Fe 0.4 The raw materials magnesium oxide, aluminum oxide, manganese dioxide and iron oxide were weighed and mixed and ground in an agate mortar for 10 hours, then calcined at 1200°C for 3 hours and ground again for 8 hours to obtain a dispersed single-phase MgO4. 0.8 Mn 0.2 Al 1.6 Fe 0.4 O4 powder;
[0026] b. The powder material obtained in step a was heated to 10 kg / cm 2 The block material is pressed at a pressure of 200 MPa for 30 seconds, and the formed block material is cold isostatically pressed at a pressure of 200 MPa for 2 minutes, and then sintered at a temperature of 1400° C. for 6 hours to obtain a disc-shaped high-density ceramic block material;
[0027] c. Coat the front and back sides of the material sintered in step b with platinum paste electrodes, and then anneal at 900°C for 30 minutes to obtain a material constant of B with a temperature range of 0-600°C. 150℃ / 550℃ =7609K, temperature 150℃ resistivity is 2.60×107 The linear fitting Pearson's r coefficient of Ω.cm, lnρ and 1000 / T is 99.99% for high temperature and wide temperature range thermistor materials;
[0028] After aging for 1000 hours at a temperature of 1000°C, the absolute value of the resistance deviation is less than 1.95%.
[0029] Example 2 (x=0.6)
[0030] a. Press Mg 0.6 Mn 0.4 Al 1.2 Fe 0.8 The raw materials magnesium oxide, aluminum oxide, manganese dioxide and iron oxide were weighed and mixed and ground in an agate mortar for 8 hours, then calcined at 1200℃ for 3 hours and ground again for 6 hours to obtain a dispersed single-phase MgO4. 0.6 Mn 0.4 Al 1.2 Fe 0.8 O4 powder;
[0031] b. The powder material obtained in step a was heated to 15 kg / cm 2 The block material is pressed at a pressure of 20 seconds, and the formed block material is cold isostatically pressed at a pressure of 250 MPa for 3 minutes, and then sintered at a temperature of 1350° C. for 5 hours to obtain a disc-shaped high-density ceramic block material;
[0032] c. Coat the front and back sides of the material sintered in step b with platinum paste electrodes, and then anneal at 900°C for 30 minutes to obtain a material constant of B with a temperature range of 0-600°C. 150℃ / 550℃ =6543K, temperature 150℃ resistivity is 5.68×10 5 The linear fitting Pearson's r coefficient of Ω.cm, lnρ and 1000 / T is 99.96% for high temperature and wide temperature range spinel thermistor materials;
[0033] After aging for 1000 hours at a temperature of 1000°C, the absolute value of the resistance deviation is less than 2.03%.
[0034] Example 3 (x=0.5)
[0035] a. Press Mg 0.5 Mn 0.5 The raw materials magnesium oxide, aluminum oxide, manganese dioxide and iron oxide were weighed and mixed and ground in an agate mortar for 9 hours, then calcined at 1100℃ for 2 hours and ground again for 7 hours to obtain a dispersed single-phase MgO 0.5 Mn 0.5 AlFeO4 powder;
[0036] b. The powder material obtained in step a was heated to 20 kg / cm 2 The block material is pressed at a pressure of 300 MPa for 20 seconds, and the formed block material is cold isostatically pressed at a pressure of 300 MPa for 2 minutes, and then sintered at a temperature of 1300° C. for 6 hours to obtain a disc-shaped high-density ceramic block material;
[0037] c. Coat the front and back sides of the material sintered in step b with platinum paste electrodes, and then anneal at 900°C for 30 minutes to obtain a material constant of B with a temperature range of 0-600°C. 150℃ / 550℃ =6357K, temperature 150℃ resistivity is 3.29×10 4 The linear fitting Pearson's r coefficient of Ω.cm, lnρ and 1000 / T is 99.98% for high temperature and wide temperature range spinel thermistor materials;
[0038] After aging for 1000 hours at a temperature of 1000°C, the absolute value of the resistance deviation is less than 1.99%.
[0039] Example 4 (x=0.4)
[0040] a. Press Mg 0.4 Mn 0.6 Al 0.8 Fe 1.2 The raw materials magnesium oxide, aluminum oxide, manganese dioxide and iron oxide were weighed and mixed and ground in an agate mortar for 9 hours, then calcined at 1150℃ for 2 hours and ground again for 7 hours to obtain a dispersed single-phase MgO4. 0.4 Mn 0.6 Al 0.8 Fe 1.2 O4 powder;
[0041] b. The powder material obtained in step a was heated to 25 kg / cm 2 The block material is pressed at a pressure of 10 seconds, and the formed block material is cold isostatically pressed at a pressure of 350 MPa for 4 minutes, and then sintered at a temperature of 1400° C. for 4 hours to obtain a disc-shaped high-density ceramic block material;
[0042] c. Coat the front and back sides of the material sintered in step b with platinum paste electrodes, and then anneal at 900°C for 30 minutes to obtain a material constant of B with a temperature range of 0-600°C. 150℃ / 550℃ =4826K, temperature 150℃, resistivity is 1.35×10 4 The linear fitting Pearson's r coefficient of Ω.cm, lnρ and 1000 / T is 99.92% for high temperature and wide temperature range spinel thermistor materials;
[0043] After aging for 1000 hours at a temperature of 1000°C, the absolute value of the resistance deviation is less than 2.21%.
[0044] Example 5 (x=0.2)
[0045] a. Press Mg 0.2 Mn 0.8 Al 0.4 Fe 1.6 The raw materials magnesium oxide, aluminum oxide, manganese dioxide and iron oxide were weighed and mixed and ground in an agate mortar for 8 hours, then calcined at 1100°C for 2 hours and ground again for 6 hours to obtain a dispersed single-phase MgO4. 0.2 Mn 0.8 Al 0.4 Fe 1.6 O4 powder;
[0046] b. The powder material obtained in step a was heated to 10 kg / cm 2 The block material is pressed at a pressure of 10 seconds, and the formed block material is cold isostatically pressed at a pressure of 200 MPa for 5 minutes, and then sintered at a temperature of 1370°C for 0.5 hours to obtain a disc-shaped high-density ceramic block material;
[0047] c. Coat the front and back sides of the material sintered in step b with platinum paste electrodes, and then anneal at 900°C for 30 minutes to obtain a material constant of B with a temperature range of 0-600°C. 150℃ / 550℃ =4383K, temperature 150℃, resistivity is 2.25×10 3 The linear fitting Pearson's r coefficient of Ω.cm, lnρ and 1000 / T is 99.76% for a high-temperature thermistor material with high stability over a wide temperature range;
[0048] After aging for 1000 hours at a temperature of 1000°C, the absolute value of the resistance deviation is less than 2.24%.
[0049] The above are only specific implementations of the present invention, but the design concept of the present invention is not limited thereto.
Claims
1. A spinel thermistor material for high temperature and wide temperature range temperature measurement, characterized in that: The thermistor material is made of magnesium oxide, aluminum oxide, manganese dioxide and iron oxide, and its chemical composition is Mg x Mn 1-x Al 2x Fe 2(1-x) O4, where 0.2≤x≤0.8, the crystal structure of the resistor material is a spinel structure, and the specific operation is carried out in the following steps: a. Press Mg x Mn 1-x Al 2x Fe 2(1-x) O4, 0.2≤x≤0.8 molar ratio, weigh the raw materials magnesium oxide, aluminum oxide, manganese dioxide and iron oxide respectively, mix and grind them in an agate mortar for 8-10 h, then calcine at a temperature of 1100-1200 ° C for 2-3 h, and grind again for 6-8 h to obtain a single-phase Mg x Mn 1-x Al 2x Fe 2(1-x) O4 powder; b. The powder material obtained in step a is heated to 10-25 Kg / cm 2 The briquetting process is carried out under a pressure of 10-30 seconds, and the formed green body is cold isostatically pressed at a pressure of 200-350 MPa for 2-5 minutes, and then sintered at a temperature of 1300-1400 ° C for 0.5-6 hours to obtain Mg x Mn 1-x Al 2x Fe 2(1-x) O4 disc-shaped high-density ceramic block material; c. Coat the front and back sides of the disc-shaped high-density ceramic block material sintered in step b with platinum slurry electrodes, and then keep it at 900°C for 30 minutes to obtain a temperature range of 0-600°C and a material constant of B 150℃ / 500℃ = 4383 K-7609 K, the resistivity is between 2.60×10 7 Ω.cm-2.25×10 3 Ω.cm, ln ρ and 1000 / T The linear fitting Pearson's r coefficient is greater than or equal to 99.76% of the high-temperature and wide-temperature range spinel thermistor materials.
2. A method for preparing a spinel thermistor material for high temperature and wide temperature range temperature measurement, characterized in that Follow these steps: a. Press Mg x Mn 1-x Al 2x Fe 2(1-x) O4, 0.2≤x≤0.8 molar ratio, weigh the raw materials magnesium oxide, aluminum oxide, manganese dioxide and iron oxide respectively, mix and grind them in an agate mortar for 8-10 h, then calcine at a temperature of 1100-1200 ° C for 2-3 h, and grind again for 6-8 h to obtain a single-phase Mg x Mn 1-x Al 2x Fe 2(1-x) O4 powder; b. The powder material obtained in step a is heated to 10-25 Kg / cm 2 The briquetting process is carried out under a pressure of 10-30 seconds, and the formed green body is subjected to cold isostatic pressing, maintained at a pressure of 200-350 MPa for 2-5 minutes, and then sintered at a temperature of 1300 ℃-1400 ℃ for 0.5-6 hours to obtain Mg x Mn 1-x Al 2x Fe 2(1-x) O4 disc-shaped high-density ceramic block material; c. Coat the front and back sides of the disc-shaped high-density ceramic block material sintered in step b with platinum slurry electrodes, and then keep it at 900°C for 30 minutes to obtain a temperature range of 0-600°C and a material constant of B 150℃ / 500℃ = 4383K-7609 K, the resistivity is between 2.60×10 7 Ω.cm-2.25×10 3 Ω.cm, ln ρ and 1000 / T The linear fitting Pearson's r coefficient is greater than or equal to 99.76% of the high-temperature and wide-temperature range spinel thermistor materials.