A superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material and preparation method thereof

By integrating SmFeO3 into a sodium bismuth titanate-based ceramic via a solid phase reaction, the material addresses low breakdown strength and curved P-E curves, achieving improved energy storage performance and efficiency, suitable for large-scale production.

CN116693285BActive Publication Date: 2024-12-03NANCHANG HANGKONG UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310576987.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-03
Estimated Expiration
2043-05-22

AI Technical Summary

Technical Problem

Existing sodium bismuth titanate (NBT) based ceramics suffer from low breakdown strength, high residual polarization, and a curved polarization-electric field (P-E) curve, limiting their energy storage performance in pulse power systems.

Method used

A superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material is developed by incorporating SmFeO3 into a binary solid solution of 0.6Na0.5Bi0.5TiO3-0.4Sr0.7Bi0.2TiO3, sintered via a solid phase reaction, with a chemical formula (1-x)(0.6Na0.5Bi0.5TiO3-0.4Sr0.7Bi0.2TiO3)-xSmFeO3, where x is between 0.05 and 0.15, using a specific preparation process involving ball milling, calcining, tableting, and sintering.

Benefits of technology

The material achieves almost zero residual polarization and a quasi-linear P-E curve, significantly enhancing discharge energy density and energy storage efficiency, with performance superior to undoped counterparts, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116693285B_ABST
    Figure CN116693285B_ABST
Patent Text Reader

Abstract

The invention discloses a superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material and a preparation method thereof. The superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material comprises a ferroelectric material component SmFeO3 and a relaxor ferroelectric material 0.6Na 0.5 Bi 0.5 TiO3‑0.4Sr 0.7 Bi 0.2 TiO3 is made by solid phase reaction sintering, and its chemical formula is (1‑x)(0.6Na 0.5 Bi 0.5 TiO3‑0.4Sr 0.7 Bi 0.2 TiO3)‑xSmFeO3, wherein x is the molar fraction, and the value range of x is 0.05≤x≤0.15. The preparation of the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material of the present invention effectively overcomes the shortcomings of high residual polarization intensity and curved P-E curve in traditional relaxor ferroelectric materials, greatly improves the discharge energy density and energy storage efficiency of the dielectric material, and the energy storage performance is significantly better than that of undoped 0.6Na 0.5 Bi 0.5 TiO3‑0.4Sr 0.7 Bi 0.2 TiO3 relaxor ferroelectric material; the preparation method of the invention has simple process, readily available raw materials, high production efficiency, and is suitable for large-scale practical production applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material technology, and in particular to a superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material and a preparation method thereof. Background Art

[0002] The high power and miniaturization of pulse power systems require the development of energy storage dielectrics with excellent performance as components. This requires the material to have a large dielectric constant, low dielectric loss and high breakdown field strength, so that the device has high energy storage density and high energy storage efficiency.

[0003] At present, most commercial energy storage materials are PbTiO3 (PT) based materials. Although pure PT ceramics have a high Curie temperature T c =490℃, but its performance is poor, and sintering is difficult, prone to cracks, and lead (Pb) is volatile, polluting the environment and endangering human health, while sodium bismuth titanate (Na 0.5 Bi 0.5 Compared with PT, TiO3, NBT) based ceramics are environmentally friendly and have cheap raw materials. The Curie temperature of NBT ceramics is as high as 320℃, and the maximum polarization intensity can exceed 45μC / cm 2 , showing excellent energy storage potential. However, NBT has the disadvantages of low breakdown strength and large residual polarization strength, making it difficult to obtain a thin and straight hysteresis loop, resulting in poor energy storage performance.

[0004] In order to improve the energy storage performance of NBT ceramics, the current methods mainly include optimizing the preparation process, element doping, and forming a binary solid solution with other stable perovskite structures. Preparation processes include: improving the sintering method or adopting a rolling process; element doping such as: lanthanum ions (La 3+ ), potassium ion (K + ), lithium ion (Li + ) doped at the A site, magnesium ions (Mg 2+ )Niobium ion (Nb 5+ Tantalum ions (Ta 5+ ) doped at the B site; and other ABO3-type ferroelectrics, such as strontium bismuth titanate (Sr 0.7 Bi 0.2 TiO3), sodium niobate (NaNbO3) and calcium titanate (CaTiO3), etc., to form a solid solution to enhance the relaxation performance. 0.7 Bi 0.2 The introduction of TiO3 makes the perovskite structure of NBT material more stable, enhances the relaxation performance and insulation performance of NBT matrix to a certain extent, and effectively reduces the residual polarization strength of the system. However, its residual polarization strength is still excessive, and more importantly, its "polarization-electric field (P-E) curve" is relatively curved, which seriously limits the improvement of its discharge energy density and energy storage efficiency.

[0005] In addition, after conducting a large amount of literature research on NBT relaxor energy storage ceramics, it was found that in addition to the conventional "enhancing polarization strength", "reducing residual polarization" and "improving breakdown strength", there is still a lack of a new path to study energy storage density, and the P-E curve directly related to energy storage density has rarely been reported. Therefore, studying the energy storage performance of NBT-based relaxor ferroelectric ceramics from the linear characteristics of the P-E curve has become an issue of great production practical significance. Summary of the invention

[0006] The purpose of the present invention is to solve the technical problems existing in the prior art and to provide a superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material and a preparation method thereof.

[0007] To achieve the above purpose, the technical solution provided by the present invention is: a superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material, the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material is composed of ferroelectric material component SmFeO3 and relaxor ferroelectric material 0.6Na 0.5 Bi 0.5 TiO3–0.4Sr 0.7 Bi 0.2 TiO3 is sintered by solid phase reaction method. The chemical formula of the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material is (1-x)(0.6Na 0.5 Bi 0.5 TiO3-0.4Sr 0.7 Bi 0.2 TiO3)–xSmFeO3, where x is the mole fraction, and x is in the range of 0.05≤x≤0.15.

[0008] The present invention also discloses a method for preparing a superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material, comprising the above-mentioned superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material, and the preparation method comprises the following steps:

[0009] Step S1: Prepare the ingredients using analytically pure Bi2O3, Na2CO3, TiO2, SrCO3, Sm2O3, and Fe2O3 as raw materials according to the preparation chemical formula (1-x)(0.6Na 0.5 Bi 0.5 TiO3-0.4Sr 0.7 Bi 0.2 TiO3)–xSmFeO3 system stoichiometric ratio Weigh the above raw materials;

[0010] Step S2: primary ball milling, placing the weighed raw materials in step S1 into a nylon ball mill, using anhydrous ethanol as a medium and zirconium oxide balls as ball milling beads, and then placing the resulting slurry in an oven and drying it at 80° C. to obtain a block powder;

[0011] Step S3: calcining, crushing the block powder dried in step S2, and grinding it in a mortar, then placing the powder ground into fine particles in a crucible for compaction, raising the temperature to 850° C. at a rate of 5° C. / min for calcining for 6 hours, and then allowing it to cool naturally to obtain a calcined powder;

[0012] Step S4: secondary ball milling, grinding the calcined powder obtained in step S3 again, and ball milling and drying again according to step S2 to obtain block powder;

[0013] Step S5: tableting, crushing the block powder obtained in step S4, adding a certain amount of PVA aqueous solution to granulate, and then placing the granulated powder in a mold for compression molding to obtain a green sheet;

[0014] Step S6: sintering into porcelain, placing the green sheet obtained in step S5 into a crucible, and covering it with the calcined powder in step S3, sintering at 1150° C.-1170° C. for two hours to obtain a porcelain-like ceramic sheet;

[0015] Step S7: Ceramic sheet electrode production: the ceramic sheet obtained by sintering in step S6 is polished and coated with gold electrodes by ion sputtering, and then subjected to electrical testing.

[0016] Preferably, in step S2, the mass ratio of the zirconia balls to the raw material is 3:1, the ball milling speed is 300 r / min, and the ball milling time is 24 hours.

[0017] Preferably, the concentration of the PVA aqueous solution used in step S5 is 3 wt %, the granulation is characterized by the powder being in the form of fine sand, the pressing method selected is cold isostatic pressing, the pressure is set to 200 MPa, and the holding time is 3 minutes.

[0018] Preferably, the sintering temperature in step S6 is specifically as follows: increasing the temperature to 500°C at 3°C / min and keeping it for 30 minutes to remove PVA, then increasing the temperature to 1150°C-1170°C at 4°C / min and keeping it for 2 hours, and finally decreasing the temperature to 650°C at 6°C / min and allowing it to cool naturally.

[0019] Beneficial effects of the present invention:

[0020] 1. The present invention can effectively overcome the shortcomings of high remanent polarization intensity and curved P-E curve in traditional relaxor ferroelectric materials, greatly improve the discharge energy density and energy storage efficiency of dielectric materials, and its performance is significantly better than that of undoped 0.6Na 0.5 Bi 0.5 TiO3-0.4Sr 0.7 Bi 0.2 TiO3 relaxor ferroelectric material.

[0021] 2. The preparation method of the present invention has simple process, readily available raw materials, high production efficiency, and is suitable for large-scale practical production applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings described herein are used to provide further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0023] Figure 1 The figure is a relationship diagram between the discharge energy density and energy storage efficiency of the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic prepared in Example 1 and the electric field intensity;

[0024] Figure 2 The hysteresis loop and nonlinear fitting curve diagram of the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic prepared in Example 1 under the breakdown electric field;

[0025] Figure 3 The figure is a relationship diagram between the discharge energy density and energy storage efficiency of the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic prepared in Example 2 and the electric field intensity;

[0026] Figure 4 The hysteresis loop and nonlinear fitting curve diagram of the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic prepared in Example 2 under the breakdown electric field;

[0027] Figure 5 The dielectric constant and dielectric loss of the superparaelectric sodium bismuth titanate-based relaxation energy storage ceramic prepared in Example 2 are plotted against temperature and frequency;

[0028] Figure 6 This is a graph showing the relationship between the energy storage performance and temperature of the superparaelectric sodium bismuth titanate-based relaxation energy storage ceramic prepared in Example 2;

[0029] Figure 7 This is a graph showing the relationship between the energy storage performance and frequency of the superparaelectric sodium bismuth titanate-based relaxation energy storage ceramic prepared in Example 2;

[0030] Figure 8 The figure is a relationship diagram between the discharge energy density and energy storage efficiency of the superparaelectric sodium bismuth titanate-based relaxation energy storage ceramic prepared in Example 3 and the electric field intensity;

[0031] Fig. 9 The hysteresis loop and nonlinear fitting curve diagram of the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic prepared in Example 3 under the breakdown electric field. DETAILED DESCRIPTION

[0032] This section will describe in detail the specific embodiments of the present invention. The preferred embodiments of the present invention are shown in the accompanying drawings. The purpose of the accompanying drawings is to supplement the description of the text part of the specification with graphics, so that people can intuitively and vividly understand each technical feature and the overall technical solution of the present invention, but it cannot be understood as a limitation on the scope of protection of the present invention.

[0033] The preferred embodiment of the present invention is a superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material, which is composed of a ferroelectric material component SmFeO3 and a relaxor ferroelectric material 0.6Na 0.5 Bi 0.5 TiO3–0.4Sr 0.7 Bi 0.2 TiO3 is sintered by solid phase reaction method. The chemical formula of the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material is (1-x)(0.6Na 0.5 Bi 0.5 TiO3–0.4Sr 0.7 Bi 0.2 TiO3)–xSmFeO3, where x is the mole fraction, and x is in the range of 0.05≤x≤0.15.

[0034] A method for preparing a superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material, comprising the above-mentioned superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material, the preparation method comprising the following steps:

[0035] Step S1: Prepare the ingredients using analytically pure Bi2O3, Na2CO3, TiO2, SrCO3, Sm2O3, and Fe2O3 as raw materials according to the preparation chemical formula (1-x)(0.6Na 0.5 Bi 0.5 TiO3-0.4Sr 0.7 Bi 0.2 TiO3)–xSmFeO3 system stoichiometric ratio Weigh the above raw materials;

[0036] Step S2: First ball milling, placing the weighed raw materials in step S1 into a nylon ball mill, using anhydrous ethanol as a medium and zirconium oxide balls as ball milling beads, wherein the total mass of the zirconium oxide ball milling beads: the total mass of the mixed raw materials = 3:1, and performing mixed ball milling for 24 hours, and then placing the obtained slurry in an oven and drying it at 80°C to obtain a block powder;

[0037] Step S3: calcining, crushing the block powder dried in step S2, and grinding it in a mortar, then placing the powder ground into fine particles in a crucible for compaction, raising the temperature to 850° C. at a rate of 5° C. / min for calcining for 6 hours, and then allowing it to cool naturally to obtain a calcined powder;

[0038] Step S4: secondary ball milling, grinding the powder calcined in step S3 again, and ball milling and drying again according to step S2 to obtain block powder;

[0039] Step S5: tableting, crushing the block powder obtained in step S4, adding a certain amount of PVA aqueous solution to granulate, and then placing the granulated powder in a mold for compression molding to obtain a green sheet;

[0040] Specifically, the concentration of the PVA aqueous solution used is 3wt%, the characteristic of the granulation is that the powder is in the form of fine sand, the pressing method selected is cold isostatic pressing, the pressure is set to 200MPa, and the holding time is 3 minutes;

[0041] Step S6: sintering into porcelain, placing the green sheet obtained in step S5 into a crucible, and covering it with the calcined powder in step S3, sintering at 1150°C-1170°C for two hours to obtain a porcelain-forming ceramic sheet;

[0042] Specifically, the sintering temperature is as follows: increasing the temperature to 500°C at 3°C / min and keeping the temperature for 30 minutes to remove PVA, then increasing the temperature to 1150°C-1170°C at 4°C / min and keeping the temperature for 2 hours, and finally decreasing the temperature to 650°C at 6°C / min and allowing it to cool naturally;

[0043] Step S7: Ceramic sheet electrode production: The ceramic sheet obtained by sintering in step S6 is polished and coated with gold electrodes by ion sputtering, and then subjected to electrical testing.

[0044] The present invention uses a typical 0.6Na 0.5 Bi 0.5 TiO3-0.4Sr 0.7 Bi 0.2 TiO3 relaxor ferroelectric ceramic material is used as the matrix, and the superparaelectric phase of the matrix is ​​regulated by doping the ferroelectric component SmFeO3. 0.5 Bi 0.5 TiO3–0.4Sr 0.7 Bi 0.2 TiO3 relaxor ferroelectric ceramic material slowly transforms from the undoped relaxor ferroelectric phase to the superparaelectric phase as the doping amount increases. The ceramic in the superparaelectric phase has ultrafine-scale nanodomains, which are more sensitive to electric fields and respond faster, and can produce almost zero residual polarization intensity and a "quasi-linear" P-E curve.

[0045] To achieve two aspects of energy storage advantages:

[0046] 1. Further reduce the remnant polarization intensity of relaxor ferroelectric to almost zero;

[0047] 2. The P-E curve of the relaxor ferroelectric bending was regulated to a quasi-linear type, further improving the discharge energy density and energy storage efficiency.

[0048] The present invention can effectively overcome the shortcomings of high remanent polarization intensity and curved P-E curve in traditional relaxor ferroelectric materials, greatly improve the discharge energy density and energy storage efficiency of dielectric materials, and its performance is significantly better than that of undoped 0.6Na 0.5 Bi 0.5 TiO3–0.4Sr 0.7 Bi 0.2 TiO3 relaxor ferroelectric material.

[0049] The preparation method of the invention has simple process, readily available raw materials and high production efficiency, and is suitable for large-scale practical production applications.

[0050] In addition, the present invention proposes for the first time the linear fitting and curvature calculation of the P–E curve to evaluate the energy storage performance.

[0051] Example 1

[0052] like Figure 1-Figure 2 The composition expression of the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic in this embodiment is as follows: 0.95(0.6Na 0.5 Bi 0.5 TiO3-0.4Sr 0.7 Bi 0.2 TiO3)–0.05SmFeO3 was prepared according to the following steps:

[0053] Step S1: preparing ingredients, using analytically pure Bi2O3, Na2CO3, TiO2, SrCO3, Sm2O3, and Fe2O3 as raw materials, and weighing corresponding masses of raw materials according to the stoichiometric ratio in the above chemical formula;

[0054] Step S2: primary ball milling, placing the weighed raw materials in step S1 into a nylon ball mill, using anhydrous ethanol as a medium and zirconium oxide balls as ball milling beads, wherein the total mass of the zirconium oxide ball milling beads: the total mass of the mixed raw materials = 3:1, and performing mixed ball milling for 24 hours, and then placing the obtained slurry in an oven and drying it at 80°C to obtain a block powder;

[0055] Step S3: calcining, crushing the block powder dried in step S2, and grinding it in a mortar, then placing the powder ground into fine particles in a crucible for compaction, raising the temperature to 850° C. at a rate of 5° C. / min for calcining for 6 hours, and then allowing it to cool naturally to obtain a calcined powder;

[0056] Step S4: secondary ball milling, grinding the powder calcined in step S3 again, and ball milling and drying again according to step S2 to obtain block powder;

[0057] Step S5: tableting, crushing the block powder obtained in step S4, adding a certain amount of PVA aqueous solution to granulate, and then placing the granulated powder in a mold for compression molding to obtain a green sheet;

[0058] Step S6: sintering into porcelain, placing the green sheet obtained in step S5 in a crucible, and covering it with the calcined powder in step S3, sintering at 1150℃-1170℃ for two hours to obtain a dense and uniformly grained superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic; the performance of the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic prepared above was tested at room temperature, and the results are shown in Table 1. The charge and discharge energy density and energy storage efficiency involved were calculated using the hysteresis loop measured by the ferroelectric analyzer Polyk, and the calculation method is:

[0059]

[0060] Among them, W, W rec , η are the charge energy density, discharge energy density and energy storage efficiency of dielectric ceramics respectively; E, P max , P r They represent the external electric field to which the dielectric ceramic is subjected, the maximum polarization intensity under the external electric field, and the residual polarization intensity after the electric field is removed.

[0061] The curvature value (K) of the hysteresis loop involved is calculated based on the fitted hysteresis loop and the maximum value is selected. The calculation method is:

[0062] K=dθ / ds=y″(x) / {1+[y′(x)] 2} 3 / 2

[0063] Among them, the relationship between discharge energy density and energy storage efficiency and electric field strength is as follows: Figure 1 As shown, the hysteresis loop under the maximum applicable electric field and the corresponding nonlinear curvature fitting curve are shown in Figure 2 As shown. 0.95(0.6Na 0.5 Bi 0.5 TiO3-0.4Sr 0.7 Bi 0.2 The maximum breakdown field strength of the TiO3)–0.05SmFeO3 system ceramic piece is 295kV / cm, and the discharge energy density is 4.7J / cm 3 , the energy storage efficiency remains above 81%, the curvature of the P–E curve is 0.29, and the specific energy storage performance and curvature parameters are shown in Table 1.

[0064] Table 1 Example 1 Superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramics performance

[0065]

[0066] Example 2

[0067] like Figure 3-Figure 7 The composition expression of the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic in this embodiment is as follows: 0.90(0.6Na 0.5 Bi 0.5 TiO3-0.4Sr 0.7 Bi 0.2 TiO3)–0.10SmFeO3 was prepared according to the following steps:

[0068] Use analytically pure Bi2O3, Na2CO3, TiO2, SrCO3, Sm2O3, and Fe2O3 as raw materials and mix them according to the stoichiometric ratio in the above chemical formula. The remaining steps are the same as in Example 1.

[0069] The experimental results are shown in Table 2, where the discharge energy storage density and energy storage efficiency vary with the electric field strength. Figure 3 As shown, the hysteresis loop under the maximum applicable electric field and the corresponding nonlinear curvature fitting curve are shown in Figure 4 The changes of dielectric constant and dielectric loss with temperature and frequency are shown in Figure 5 As shown in the figure, the energy storage performance obtained by the 200kV / cm test varies with temperature. Figure 6 As shown in the figure, the energy storage performance obtained by the 300kV / cm test varies with frequency. Figure 7 As shown in the figure, 0.90(0.6Na 0.5 Bi 0.5 TiO3-0.4Sr 0.7 Bi 0.2 The maximum breakdown field strength of the TiO3)–0.10SmFeO3 system ceramic sheet can reach 430kV / cm, and the discharge energy density can reach 7.2J / cm 3 The energy storage efficiency is over 86%, the curvature of the hysteresis loop is 0.02, and the degree of linearity is greatly enhanced. The specific performance is shown in Table 2.

[0070] Table 2 Performance of superparaelectric sodium bismuth titanate-based relaxation energy storage ceramics in Example 2

[0071]

[0072] Embodiment 3,

[0073] As 8- Fig. 9 The composition expression of the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic in this embodiment is as follows: 0.85(0.6Na 0.5 Bi 0.5 TiO3–0.4Sr 0.7Bi 0.2 TiO3)–0.15SmFeO3 was prepared according to the following steps:

[0074] Use analytically pure Bi2O3, Na2CO3, TiO2, SrCO3, Sm2O3, and Fe2O3 as raw materials and mix them according to the stoichiometric ratio in the above chemical formula. The remaining steps are the same as in Example 1.

[0075] The experimental results are shown in Table 3, where the discharge energy density and energy storage efficiency vary with the electric field strength. Figure 8 As shown, the hysteresis loop under the maximum applicable electric field and the corresponding nonlinear curvature fitting curve are shown in Fig. 9 As shown. 0.85(0.6Na 0.5 Bi 0.5 TiO3–0.4Sr 0.7 Bi 0.2 The maximum breakdown field strength of the TiO3)–0.15SmFeO3 system ceramic piece is 322kV / cm, and the discharge energy density is 3.27J / cm 3 , the energy storage efficiency is as high as 92% and the curvature is 6.5×10 -7 , the hysteresis loop is almost close to a straight line. The specific performance is shown in Table 2.

[0076] Table 3 Performance of superparaelectric sodium bismuth titanate-based relaxation energy storage ceramics in Example 3

[0077]

[0078] Under the premise that no conflict occurs, those skilled in the art may freely combine and superimpose the above-mentioned additional technical features.

[0079] The above description is only a preferred implementation mode of the present invention. Any technical solution that achieves the purpose of the present invention by substantially the same means belongs to the protection scope of the present invention.

Claims

1. A superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material, Features: The chemical formula of the superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material is (1-x)(0.6Na 0.5 Bi 0.5 TiO 3 –0.4Sr 0.7 Bi 0.2 TiO 3 )–xSmFeO 3 , wherein x is the mole fraction, and x is in the range of 0.1≤x≤0.15, and the preparation method comprises the following steps: Step S1: Prepare analytically pure Bi 2 O 3 、Na 2 CO 3 、TiO 2 、SrCO 3 、Sm 2 O 3 , Fe 2 O 3 As raw materials, the preparation chemical formula is (1-x)(0.6Na 0.5 Bi 0.5 TiO 3 –0.4Sr 0.7 Bi 0.2 TiO 3 )–xSmFeO 3 Weigh the above raw materials according to the system stoichiometric ratio; Step S2: primary ball milling, placing the weighed raw materials in step S1 into a nylon ball mill, using anhydrous ethanol as a medium and zirconium oxide balls as ball milling beads, and then placing the resulting slurry in an oven and drying it at 80° C. to obtain a block powder; Step S3: calcining, crushing the block powder dried in step S2, and grinding it in a mortar, then placing the powder ground into fine particles in a crucible for compaction, raising the temperature to 850° C. at a rate of 5° C. / min for calcining for 6 hours, and then allowing it to cool naturally to obtain a calcined powder; Step S4: secondary ball milling, grinding the calcined powder obtained in step S3 again, and ball milling and drying again according to step S2 to obtain block powder; Step S5: tableting, crushing the block powder obtained in step S4, adding a certain amount of PVA aqueous solution to granulate, and then placing the granulated powder in a mold for compression molding to obtain a green sheet; Step S6: sintering into porcelain, placing the green sheet obtained in step S5 in a crucible, and covering it with the calcined powder in step S3, raising the temperature to 500°C at 3°C / min and keeping it for 30 minutes to remove PVA, then raising the temperature to 1150°C-1170°C at 4°C / min and keeping it for 2 hours, and finally lowering the temperature to 650°C at 6°C / min and letting it cool naturally; Step S7: Ceramic sheet electrode production: The ceramic sheet obtained by sintering in step S6 is polished and coated with gold electrodes by ion sputtering, and then subjected to electrical testing.

2. A superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material according to claim 1, Features: In step S2, the mass ratio of the zirconia balls to the raw materials is 3:1, the ball milling speed is 300 r / min, and the ball milling time is 24 hours.

3. A superparaelectric phase sodium bismuth titanate-based relaxation energy storage ceramic material according to claim 1, Features: The concentration of the PVA aqueous solution used in step S5 is 3 wt %. The characteristic of the completed granulation is that the powder is in the form of fine sand. The pressing method selected is cold isostatic pressing, the pressure is set to 200 MPa, and the holding time is 3 minutes.