A high thermal conductivity solvent-free thermal conductive silicone grease and preparation method thereof
Through the use of low-viscosity alcohol hydroxy silicone oil, linear polydimethylsiloxane compound and silicon carbide-alumina composite, the contradiction between thermal grease viscosity and thermal conductivity is solved, and high thermal conductivity and stability are achieved. Avoid instability caused by solvents.
Patent Information
- Application Number
- CN202310795310.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-30
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-06-30
AI Technical Summary
When existing thermal greases increase the fill amount of thermal powder, increasing viscosity leads to printing difficulties and degradation of thermal conductivity, and adding solvents to adjust viscosity will lead to instability and volatility, which leads to application difficulties.
Low viscosity alcohol hydroxy silicone oil is used to combine linear polydimethylsiloxane, combining thermal conductor powder with different particle sizes and silicon carbide-alumina composites to improve phase interface and reduce friction and improve The filling amount and dispersion of the thermally conductive powder form a stable thermal conductivity path.
The high thermal conductivity is maintained and the viscosity is moderate, the stability and uniformity of thermal grease are ensured, the instability and volatility caused by the use of solvents are avoided, and the use performance of thermal grease is improved.
Abstract
Description
Technical Field
[0001] The invention relates to the field of thermal conductive silicone grease, and in particular to a highly thermal conductive solvent-free thermal conductive silicone grease and a preparation method thereof. Background Art
[0002] Thermal grease is a highly thermally conductive insulating silicone material that can maintain its grease state for a long time at a temperature of -50℃-230℃. It has both excellent electrical insulation and excellent thermal conductivity. It also has low freeness (tending to zero), is resistant to high and low temperatures, water, ozone, and weathering. It can be widely applied to various electronic products.
[0003] In order to achieve a higher thermal conductivity coefficient of thermal grease, the general treatment method is to fill more thermal powder. In this way, the viscosity of the thermal grease increases with the increase of the filling amount of thermal powder. However, too high viscosity will cause printing difficulties. In addition, the greater the filling amount of thermal powder, the greater the viscosity of the thermal grease, which will lead to poor wettability of the powder surface. When there is not enough silicone oil to wrap the powder, increasing the powder filling amount and the air interface between the silicone oil will cause the thermal chain to partially break, which will also make the thermal conductivity of the thermal grease worse. In order to solve this problem, solvents are generally added to adjust the viscosity of the thermal grease to improve the applicability of the thermal grease.
[0004] Adding solvent is only a stopgap measure, which can easily cause instability of thermal grease. For example, during storage and transportation, the solvent is easy to evaporate and stratify, causing the viscosity of the thermal grease to increase, and even agglomeration, resulting in difficulty in application or inability to use. In addition, after use, if the solvent is not evaporated in time, during the use of the device, the solvent will evaporate and escape again, causing holes or bubbles to form in the middle of the thermal grease, resulting in an incomplete thermal interface, thus affecting the heat dissipation of the device.
[0005] Therefore, how to reduce the use of solvents while ensuring that the thermal grease has a high filling amount of thermal conductive powder is a problem that needs to be solved. Summary of the invention
[0006] In order to reduce the use of solvents while ensuring that the thermal grease has a higher thermal conductivity, the present application provides a highly thermally conductive solvent-free thermal grease and a preparation method thereof.
[0007] In a first aspect, the present application provides a highly thermally conductive solvent-free thermally conductive silicone grease, which adopts the following technical solution:
[0008] A highly thermally conductive solvent-free thermally conductive silicone grease comprising the following raw materials:
[0009] Linear polydimethylsiloxane 30-50 parts;
[0010] 6-10 parts of alcohol hydroxy silicone oil;
[0011] Silane coupling agent 2-8 parts;
[0012] Dispersant 2-8 parts;
[0013] Thermal conductive powder 450-700 parts;
[0014] The viscosity of alcohol hydroxy silicone oil is lower than that of linear polydimethylsiloxane.
[0015] By adopting the above technical solution, in order to improve the thermal conductivity of thermal grease, more thermal conductive powder is generally filled. The linear structure of linear polydimethylsiloxane can effectively wrap the thermal conductive powder, so that the thermal conductive powder can form a stable and effective thermal conductive path in the system.
[0016] However, the applicant has found that the filling of more thermally conductive powder and the high viscosity of linear polydimethylsiloxane make the viscosity of thermal grease relatively high. When in use, the fluidity of thermal grease is poor, and problems such as uneven coating and clogging occur. The compounding of alcohol hydroxy silicone oil with lower viscosity and linear polydimethylsiloxane can obtain a thermal grease with moderate viscosity, good thermal conductive powder filling effect, and more stable performance of thermal grease. The alcohol hydroxy silicone oil with lower viscosity is directly compounded with polydimethylsiloxane, which can directly reduce the viscosity of thermal grease and increase the filling amount of thermal conductive powder. In addition, the organic functional group alcohol hydroxyl contained in the alcohol hydroxy silicone oil can improve the phase interface between thermal conductive powder and system, reduce the friction between thermal conductive powder, reduce the viscosity of the system, and further increase the filling amount of thermal conductive powder.
[0017] In addition, the applicant has found that if high and low viscosity polydimethylsiloxanes are selected for compounding, although the viscosity of the thermal grease is reduced and the filling amount of the thermally conductive powder can be appropriately increased, the thermally conductive powder is prone to uneven dispersion and agglomeration. Analysis shows that this may be because all the organic groups of polydimethylsiloxane are methyl groups, which cannot effectively improve the compatibility of the thermally conductive powder with the system, and thus the thermally conductive powder is prone to agglomeration, affecting the thermal conductivity of the thermal grease.
[0018] In a specific embodiment, at 25°C, the viscosity of the linear polydimethylsiloxane is 350 cs, and the viscosity of the alcohol hydroxy silicone oil is 40-130 mm 2 / s.
[0019] By adopting the above technical solution, the viscosity of the thermal grease is reduced by adding alcohol hydroxy silicone oil with lower viscosity, thereby increasing the filling amount of the thermally conductive powder, and making it easier to evenly disperse the thermally conductive powder in the thermally conductive grease during mixing, thereby improving the thermal conductivity of the thermally conductive grease.
[0020] In a specific embodiment, the thermally conductive powder comprises aluminum oxide and aluminum nitride in a mass ratio of (2-3):1, the particle size of the aluminum oxide is 8-15 μm, and the particle size of the aluminum nitride is 1-3 μm.
[0021] By adopting the above technical solution, thermal conductive powders of different particle sizes are selected to be filled in the thermal conductive silicone grease, and small-particle thermal conductive powders are filled between large-particle thermal conductive powders, which helps to form an effective thermal conductive path, so that the thermal conductive silicone grease has a better thermal conductive effect.
[0022] In a specific embodiment, the thermally conductive powder comprises aluminum oxide, silicon carbide-aluminum oxide composite and aluminum nitride in a mass ratio of (8-10):(3-5):1, and the silicon carbide-aluminum oxide composite is a composite of silicon carbide whiskers and aluminum oxide.
[0023] By adopting the above technical solution, the thermal conductivity of silicon carbide whiskers is higher than that of aluminum oxide, and the thermal conductivity of silicon carbide can reach 10 times that of aluminum oxide. Selecting to fill silicon carbide whiskers in thermal grease can effectively increase the thermal conductivity of thermal grease, but at the same time, the hardness of silicon carbide whiskers is higher than that of aluminum oxide. After adding silicon carbide whiskers, the hardness of thermal grease will increase relatively. If the hardness of thermal grease is too large, it will affect the fit between thermal grease and materials. The worse the fit, the lower the heat transfer efficiency between thermal grease and materials. Therefore, the applicant combines silicon carbide whiskers and aluminum oxide, and in the thermal grease system, with the help of the rapid heat conduction of silicon carbide, the thermal grease can quickly transfer the heat generated by the material, while improving the thermal conductivity of thermal grease, and ensuring that the thermal grease and materials can be effectively fit.
[0024] In a specific embodiment, the silicon carbide-aluminum oxide composite is prepared as follows:
[0025] Alumina, silicon carbide whiskers, sodium polyacrylate and water are mixed and ball-milled, spray-granulated after ball-milling, and sintered at 500-550° C. to obtain primary powder; the mass ratio of alumina, silicon carbide whiskers, sodium polyacrylate and water is (8-10):(12-15):2:1;
[0026] The primary powder and the polyvinyl alcohol aqueous solution are mixed in a mass ratio of (3-5):1 and ball-milled, spray-granulated after ball-milling, and sintered at 550-600°C to obtain a silicon carbide-aluminum oxide composite.
[0027] By adopting the above technical solution, silicon carbide whiskers are compounded on alumina. In the thermal grease, the silicon carbide whiskers on the surface of alumina can quickly transfer heat to the thermal powder in contact with it, so that heat can be quickly transferred in the thermal grease, which shows that the thermal grease has excellent thermal conductivity. At the same time, compared with directly adding silicon carbide particles, the method of compounding silicon carbide whiskers and alumina is not likely to cause a significant increase in the hardness of the thermal grease, so that the thermal grease and the material can be effectively bonded.
[0028] In a specific embodiment, the silicon carbide whisker has a length of 5-8 μm and a diameter of 0.1-0.6 μm, and the alumina is spherical alumina with a particle size of 8-15 μm.
[0029] By adopting the above technical solution, the applicant found that silicon carbide whiskers of a specific length and a specific diameter are easy to be compounded on the surface of alumina. If the length is too long, protruding silicon carbide whiskers are easy to appear on the surface of the formed silicon carbide-alumina composite, resulting in the silicon carbide-alumina composite not being easy to be evenly dispersed in the thermal grease during mixing; if the length is too short, the silicon carbide whiskers are difficult to be evenly compounded on the surface of alumina, thereby affecting the thermal conductivity between the silicon carbide-alumina composite and other thermal conductive powders. However, the silicon carbide whiskers of a specific length and a specific diameter are selected to be compounded with alumina, and the silicon carbide-alumina composite prepared is added to the thermal grease to effectively improve the thermal conductivity of the thermal grease.
[0030] In a specific embodiment, the silane coupling agent is KH550 or KH560.
[0031] By adopting the above technical solution, the thermally conductive powder is promoted to be evenly dispersed in the thermally conductive silicone grease, so that the thermally conductive powder forms an effective thermal conductive path in the thermally conductive silicone grease.
[0032] In a second aspect, the present application provides a method for preparing a highly thermally conductive solvent-free thermally conductive silicone grease, using the following technical solution:
[0033] A method for preparing a high thermal conductivity solvent-free thermal conductive silicone grease comprises the following steps: firstly mixing linear polydimethylsiloxane, alcohol hydroxy silicone oil and a dispersant according to a raw material ratio; then adding a silane coupling agent and a thermal conductive powder, and mixing them to obtain a high thermal conductivity solvent-free thermal conductive silicone grease.
[0034] In a specific embodiment, when mixing the raw materials, the stirring speed is 5-30 r / min.
[0035] By adopting the above technical solution, a highly thermally conductive solvent-free thermally conductive silicone grease is prepared.
[0036] In summary, the present application includes at least one of the following beneficial technical effects:
[0037] 1. This application selects low-viscosity alcohol hydroxy silicone oil and linear polydimethylsiloxane for compounding, which can achieve the purpose of reducing the viscosity of thermal conductive silicone grease and increasing the filling amount of thermal conductive powder;
[0038] 2. In the present application, silicon carbide whiskers are compounded with aluminum oxide and then added into thermal grease. The excellent thermal conductivity of silicon carbide whiskers can effectively improve the thermal conductivity of thermal grease. DETAILED DESCRIPTION
[0039] The present application is further described in detail below in conjunction with Example 1.
[0040] The raw materials in this application are all commercially available, among which the linear polydimethylsiloxane with a viscosity of 350cs is branded as Shin-Etsu KF-96-350cs; the linear polydimethylsiloxane with a viscosity of 100cs is branded as Shin-Etsu KF-96-100cs; the viscosity of 130mm 2 / s alcohol hydroxy silicone oil is Shin-Etsu X-22-176DX; viscosity is 40mm 2 / s alcohol hydroxy silicone oil is Shin-Etsu X-22-170BX; viscosity is 65mm 2 The alcohol hydroxy silicone oil with a content of / s is Shin-Etsu X-22-170DX; the dispersant is BYK-LP X21879.
[0041] Preparation Example 1
[0042] Accurately weigh alumina, silicon carbide whiskers, sodium polyacrylate and water, the alumina particle size is 15 μm, the silicon carbide whiskers are 8 μm in length and 0.6 μm in diameter, alumina, silicon carbide whiskers, sodium polyacrylate and water are mixed at a mass ratio of 8:12:2:1 and ball-to-material ratio is 15:1, spray granulation is performed after ball milling, and sintering is performed at 500°C for 5 min to obtain primary powder;
[0043] The primary powder and a polyvinyl alcohol aqueous solution with a mass concentration of 6wt% were mixed in a mass ratio of 3:1 and ball-milled for 2h, with a ball-to-material ratio of 15:1. After ball milling, spray granulation was performed and sintered at 550°C for 5min to obtain a silicon carbide-alumina composite.
[0044] Preparation Example 2
[0045] Accurately weigh alumina, silicon carbide whiskers, sodium polyacrylate and water, the alumina particle size is 8 μm, the silicon carbide whiskers are 5 μm in length and 0.1 μm in diameter, alumina, silicon carbide whiskers, sodium polyacrylate and water are mixed at a mass ratio of 10:15:2:1 and ball-to-material ratio is 15:1, spray granulation is performed after ball milling, and sintering is performed at 550°C for 5 min to obtain primary powder;
[0046] The primary powder and a polyvinyl alcohol aqueous solution with a mass concentration of 6wt% were mixed in a mass ratio of 5:1 and ball-milled for 2h, with a ball-to-material ratio of 15:1. After ball milling, spray granulation was performed and sintered at 600°C for 5min to obtain a silicon carbide-alumina composite.
[0047] Preparation Example 3
[0048] Accurately weigh alumina, silicon carbide whiskers, sodium polyacrylate and water, the particle size of alumina is 15 μm, the length of silicon carbide whiskers is 15 μm and the diameter is 1 μm, mix alumina, silicon carbide whiskers, sodium polyacrylate and water in a mass ratio of 8:12:2:1 and ball mill for 2 h, the ball-to-material ratio is 15:1, spray granulation is performed after ball milling, and sintering is performed at 500°C for 5 min to obtain primary powder; mix the primary powder and a polyvinyl alcohol aqueous solution with a mass concentration of 6 wt% in a mass ratio of 3:1 and ball mill for 2 h, the ball-to-material ratio is 15:1, spray granulation is performed after ball milling, and sintering is performed at 550°C for 5 min to obtain a silicon carbide-alumina composite.
[0049] Example 1
[0050] A highly thermally conductive solvent-free thermal grease, comprising 300 g of linear polydimethylsiloxane with a viscosity of 350 cs, 80 g of a 2 / s alcohol hydroxy silicone oil, 20g silane coupling agent, 20g dispersant and 480g thermal conductive powder. The thermal conductive powder is aluminum oxide with a particle size of 8-15μm.
[0051] During the preparation, linear polydimethylsiloxane, alcohol hydroxy silicone oil and dispersant are mixed and stirred at a speed of 5r / min for 30min; then silane coupling agent and thermal conductive powder are added and stirred at a speed of 5r / min for 1h to obtain high thermal conductivity solvent-free thermal conductive silicone grease.
[0052] Example 2
[0053] A highly thermally conductive solvent-free thermal grease, comprising 400 g of linear polydimethylsiloxane with a viscosity of 350 cs, 60 g of a 2 / s alcohol hydroxy silicone oil, 40g silane coupling agent, 40g dispersant and 450g thermal conductive powder. The thermal conductive powder is aluminum oxide with a particle size of 8-15μm.
[0054] During the preparation, linear polydimethylsiloxane, alcohol hydroxy silicone oil and dispersant are mixed, and stirred at a speed of 30 r / min for 30 minutes; then, silane coupling agent and thermal conductive powder are added, and stirred at a speed of 30 r / min for 1 hour to obtain high thermal conductivity solvent-free thermal conductive silicone grease.
[0055] Example 3
[0056] A highly thermally conductive solvent-free thermal grease, comprising 500 g of linear polydimethylsiloxane with a viscosity of 350 cs, 100 g of a polysiloxane with a viscosity of 65 mm 2 / s alcohol hydroxy silicone oil, 80g silane coupling agent, 80g dispersant and 700g thermal conductive powder. The thermal conductive powder is aluminum oxide with a particle size of 8-15μm.
[0057] During the preparation, linear polydimethylsiloxane, alcohol hydroxy silicone oil and dispersant are mixed and stirred at a speed of 5r / min for 30min; then silane coupling agent and thermal conductive powder are added and stirred at a speed of 5r / min for 1h to obtain high thermal conductivity solvent-free thermal conductive silicone grease.
[0058] Example 4
[0059] The difference between this embodiment and embodiment 1 is that a highly thermally conductive solvent-free thermally conductive silicone grease comprises 300 g of linear polydimethylsiloxane with a viscosity of 350 cs, 80 g of a polydimethylsiloxane with a viscosity of 130 mm 2 / s of alcohol hydroxy silicone oil, 20g of silane coupling agent, 20g of dispersant and 450g of thermal conductive powder.
[0060] Example 5
[0061] The difference between this embodiment and embodiment 1 is that a highly thermally conductive solvent-free thermally conductive silicone grease comprises 300 g of linear polydimethylsiloxane with a viscosity of 350 cs, 80 g of a polydimethylsiloxane with a viscosity of 130 mm 2 / s of alcohol hydroxy silicone oil, 20g of silane coupling agent, 20g of dispersant and 600g of thermal conductive powder.
[0062] Example 6
[0063] The difference between this embodiment and embodiment 1 is that a highly thermally conductive solvent-free thermally conductive silicone grease comprises 300 g of linear polydimethylsiloxane with a viscosity of 350 cs, 80 g of a polydimethylsiloxane with a viscosity of 130 mm 2 / s of alcohol hydroxy silicone oil, 20g of silane coupling agent, 20g of dispersant and 700g of thermal conductive powder.
[0064] Example 7
[0065] The difference between this embodiment and embodiment 1 is that the thermal conductive powder is composed of aluminum oxide and aluminum nitride in a mass ratio of 2:1, the particle size of the aluminum oxide is 8-15 μm, and the particle size of the aluminum nitride is 1-3 μm.
[0066] Example 8
[0067] The difference between this embodiment and embodiment 1 is that the thermal conductive powder is composed of aluminum oxide and aluminum nitride in a mass ratio of 3:1, the particle size of the aluminum oxide is 8-15 μm, and the particle size of the aluminum nitride is 1-3 μm.
[0068] Example 9
[0069] The difference between this embodiment and embodiment 1 is that the thermal conductive powder is composed of aluminum oxide, silicon carbide-aluminum oxide composite and aluminum nitride in a mass ratio of 8:3:1, the aluminum oxide particle size is 8-15 μm, the aluminum nitride particle size is 1-3 μm, and the silicon carbide-aluminum oxide composite is selected from Preparation Example 1.
[0070] Example 10
[0071] The difference between this embodiment and embodiment 1 is that the thermal conductive powder is composed of aluminum oxide, silicon carbide-aluminum oxide composite and aluminum nitride in a mass ratio of 10:5:1, the aluminum oxide particle size is 8-15 μm, the aluminum nitride particle size is 1-3 μm, and the silicon carbide-aluminum oxide composite is selected from Preparation Example 1.
[0072] Embodiment 11
[0073] The difference between this embodiment and embodiment 1 is that the thermal conductive powder is composed of aluminum oxide, silicon carbide-aluminum oxide composite and aluminum nitride in a mass ratio of 8:3:1, the aluminum oxide particle size is 8-15 μm, the aluminum nitride particle size is 1-3 μm, and the silicon carbide-aluminum oxide composite is selected from Preparation Example 2.
[0074] Example 12
[0075] The difference between this embodiment and embodiment 1 is that the thermal conductive powder is composed of aluminum oxide, silicon carbide-aluminum oxide composite and aluminum nitride in a mass ratio of 8:3:1, the aluminum oxide particle size is 8-15 μm, the aluminum nitride particle size is 1-3 μm, and the silicon carbide-aluminum oxide composite is selected from Preparation Example 3.
[0076] Comparative Example 1
[0077] The difference between this comparative example and embodiment 1 is that a highly thermally conductive solvent-free thermally conductive silicone grease includes 300 g of linear polydimethylsiloxane with a viscosity of 350 cs, 80 g of linear polydimethylsiloxane with a viscosity of 100 cs, 20 g of a silane coupling agent, 20 g of a dispersant, and 480 g of a thermally conductive powder. The thermally conductive powder is aluminum oxide with a particle size of 8-15 μm.
[0078] Comparative Example 2
[0079] The difference between this comparative example and embodiment 1 is that a highly thermally conductive solvent-free thermally conductive silicone grease includes 300 g of linear polydimethylsiloxane with a viscosity of 350 cs, 80 g of linear polydimethylsiloxane with a viscosity of 100 cs, 20 g of a silane coupling agent, 20 g of a dispersant, and 600 g of a thermally conductive powder. The thermally conductive powder is aluminum oxide with a particle size of 8-15 μm.
[0080] Comparative Example 3
[0081] The difference between this comparative example and embodiment 1 is that a highly thermally conductive solvent-free thermally conductive silicone grease includes 300 g of linear polydimethylsiloxane with a viscosity of 350 cs, 80 g of linear polydimethylsiloxane with a viscosity of 100 cs, 20 g of a silane coupling agent, 20 g of a dispersant, and 700 g of a thermally conductive powder. The thermally conductive powder is aluminum oxide with a particle size of 8-15 μm.
[0082] Performance Testing
[0083] The thermal conductive silicone grease in each embodiment and comparative example was poured into a 3 cm thick mold, a packaging film was covered on the thermal conductive silicone grease, and then the thermal conductivity of the thermal conductive silicone grease was measured using a QTM-500 thermal conductivity meter. After the test, the thermal conductive silicone grease was placed in a high temperature and high humidity environment, specifically, the thermal conductive silicone grease was placed in an atmosphere of pressure and 130°C / 85% relative humidity for 90 hours, and then the thermal conductivity of the thermal conductive silicone grease was measured using a QTM-500 thermal conductivity meter.
[0084] Table 1 Performance test results
[0085] project Thermal conductivity (W / (m·K)) Thermal conductivity after high temperature and high humidity (W / (m·K)) Example 1 5.7 5.3 Example 2 5.5 5.1 Example 3 5.8 5.5 Example 4 5.3 4.9 Example 5 5.9 5.6 Example 6 6.1 5.7 Example 7 6.0 5.7 Example 8 6.2 5.9 Example 9 6.4 6.0 Example 10 6.5 6.2 Embodiment 11 6.6 6.3 Example 12 5.9 5.5 Comparative Example 1 5.6 4.9 Comparative Example 2 5.8 5.3 Comparative Example 3 5.7 5.1
[0086] Referring to Table 1, compared with Comparative Examples 1 to 3, the thermal grease in Examples 1 to 3 has a better thermal conductivity, and after being subjected to a high temperature and high humidity environment, the thermal conductivity of the thermal grease is still better than that of Comparative Example 1, showing better durability in use. It is analyzed that the present application selects linear polydimethylsiloxane and lower viscosity alcohol hydroxy silicone oil to prepare thermal grease, so that the viscosity of the thermal grease is relatively low, and more thermal conductive powder can be filled, so that the thermal grease has better thermal conductivity. After replacing the alcohol hydroxy silicone oil with low viscosity linear polydimethylsiloxane, after being subjected to a high temperature and high humidity environment, the thermal conductivity of the thermal grease shows a significant decrease, and as the filling amount of the thermal conductive powder increases, the thermal conductivity of the thermal grease decreases after being appropriately improved. Analysis shows that compared with silicone oil containing alcoholic hydroxyl groups, polydimethylsiloxane whose organic groups are all methyl groups has a relatively weaker effect on improving the compatibility between thermal conductive powder and the system, thereby weakening the formation of thermal conductive pathways, which in turn manifests as a decrease in the thermal conductivity of the thermal grease.
[0087] In combination with Example 1, Example 7 and Example 8, the thermal conductivity of the thermal grease in Example 1 is relatively weak, indicating that powders of different particle sizes are selected for compounding. In the thermal grease, small-particle powders are filled between large-particle powders, and the large and small particles are in effective contact, thereby forming an effective heat conduction path, which is manifested as the thermal grease having better thermal conductivity.
[0088] In combination with Example 1 and Example 9 to Example 12, the thermal grease in Example 9 to Example 12 exhibits better thermal conductivity, indicating that the thermal conductivity of the thermal grease can be improved by compounding silicon carbide whiskers and aluminum oxide with the help of the excellent thermal conductivity of silicon carbide whiskers. At the same time, compared with directly adding silicon carbide particles, the use of silicon carbide whiskers and aluminum oxide composites can ensure that the hardness of the thermal grease is moderate, so that the thermal grease can better fit the material, thereby enabling the thermal grease to effectively transfer heat.
[0089] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A highly thermally conductive solvent-free thermal grease, characterized in that: Including the following ingredients: Linear polydimethylsiloxane 30-50 parts; 6-10 parts of alcohol hydroxy silicone oil; Silane coupling agent 2-8 parts; Dispersant 2-8 parts; Thermal conductive powder 450-700 parts; The viscosity of alcohol hydroxy silicone oil is less than that of linear polydimethylsiloxane; The thermally conductive powder comprises aluminum oxide, a silicon carbide-aluminum oxide composite and aluminum nitride in a mass ratio of (8-10): (3-5): 1, wherein the silicon carbide-aluminum oxide composite is a composite of silicon carbide whiskers and aluminum oxide; The preparation of the silicon carbide-aluminum oxide composite is as follows: Aluminum oxide, silicon carbide whiskers, sodium polyacrylate and water are mixed and ball-milled, spray-granulated after ball-milling, and sintered at 500-550°C to obtain primary powder; the mass ratio of aluminum oxide, silicon carbide whiskers, sodium polyacrylate and water is (8-10): (12-15): 2:1; The primary powder and the polyvinyl alcohol aqueous solution are mixed in a mass ratio of (3-5):1 and ball-milled, spray-granulated after ball-milling, and sintered at 550-600° C. to obtain a silicon carbide-aluminum oxide composite; The silicon carbide whisker has a length of 5-8 μm and a diameter of 0.1-0.6 μm, and the alumina is spherical alumina with a particle size of 8-15 μm.
2. The highly thermally conductive solvent-free thermally conductive silicone grease according to claim 1, characterized in that: At 25°C, the viscosity of the linear polydimethylsiloxane is 350cs, and the viscosity of the alcohol hydroxy silicone oil is 40-130mm 2 / s.
3. The highly thermally conductive solvent-free thermally conductive silicone grease according to claim 1, characterized in that: The silane coupling agent is KH550 or KH560.
4. A method for preparing a highly thermally conductive solvent-free thermally conductive silicone grease according to any one of claims 1 to 3, characterized in that: According to the raw material ratio, linear polydimethylsiloxane, alcohol hydroxy silicone oil and dispersant are first mixed; then silane coupling agent and thermal conductive powder are added and mixed to obtain high thermal conductivity solvent-free thermal conductive silicone grease.
5. The method for preparing a highly thermally conductive solvent-free thermally conductive silicone grease according to claim 4, characterized in that: When mixing the raw materials, the stirring speed is 5-30r / min.