A front silver-aluminum paste for TOPCon solar cells and its preparation method and application

By using silver-aluminum conductive slurry compounded with resin and dispersant in TOPCon solar cells, the problem of poor mesh penetration of the conductive slurry is solved, higher cell conversion efficiency and thin-line electrodes are achieved, which is suitable for narrow Small line diameter opening printing screen.

CN116779212BActive Publication Date: 2024-10-29DK ELECTRONICS MATERIALS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310710627.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-15
Publication Date
2024-10-29
Estimated Expiration
2043-06-15

AI Technical Summary

Technical Problem

The front-side conductive paste of existing TOPCon solar cells has poor screen passability, resulting in low cell conversion efficiency, and is not suitable for the mass production needs of narrow wire diameter and small opening printing screens.

Method used

A silver-aluminum conductive paste containing 80-95wt% conductive powder, 0.1-7wt% glass powder and 1.5-15wt% organic carrier paste is used, and compound resin and dispersant are used for coating and dispersion to reduce the amount of powder Reunion, improve ink transfer and bonding strength, suitable for narrow line diameter and small opening printing screen.

Benefits of technology

It achieves better ink passing performance and thinner electrode lines, reduces electrode resistance, improves the photoelectric conversion efficiency of solar cells and the printing operation window, and is suitable for narrow line width opening printing screens.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116779212B_ABST
    Figure CN116779212B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of solar cells, and specifically discloses a front silver-aluminum paste for TOPCon solar cells, a preparation method thereof, and an application thereof. The conductive silver-aluminum paste comprises 80-95wt% of conductive powder, 0.1-7wt% of glass powder, and 1.5-15wt% of an organic carrier paste composition, wherein the organic carrier paste composition comprises a compounded resin, a compounded dispersant, an organic solvent, and an additive. The compounded resin and the compounded dispersant can effectively solve the problem that the conductive silver-aluminum paste has high solid content and viscosity, poor ink passing properties, and thus leads to poor mass production yield and conversion efficiency of batteries on narrow line width screens.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solar cells, and in particular to a thin-line silver-aluminum conductive paste, a front silver-aluminum paste of a tunneling oxide passivated contact crystalline silicon solar cell (Tunnel Oxide Passivated Contact, TOPCon), and a preparation method and application thereof. Background Art

[0002] The front light-receiving surface of the silicon wafer of the solar cell has a conductive sub-grid electrode, which reduces the light-receiving area of ​​the silicon wafer and affects the efficiency. Therefore, it is hoped that a finer electrode can be formed on the front light-receiving surface of the silicon wafer to increase the light-receiving area and thus improve the photovoltaic conversion efficiency of the cell. In the existing mass production technology, the tendency is to use a narrower opening screen printing screen technology to produce electrodes in large quantities and quickly. The fine-line grid electrode obtained by this technology has a relatively small light-shielding area on the silicon wafer, so it can obtain a higher photocurrent and further obtain better photovoltaic conversion efficiency. In addition, the narrower opening screen design is also in line with the trend of overcoming the demand cost reduction, and can simultaneously meet the needs of reducing costs and improving efficiency in the industry, achieving the optimal price-performance ratio.

[0003] Compared with the currently mass-produced PERC cell structure, the new generation of TOPCon tunneling oxide passivated contact crystalline silicon solar cells has a back passivation achieved by an ultra-thin tunneling oxide layer and a doped polysilicon layer. The electrode is only in contact with the polysilicon layer, and the carrier conduction uses the tunneling effect to avoid serious metal-semiconductor recombination, which can effectively improve the cell conversion efficiency. Among them, the TOPCon front conductive paste uses two conductive powders, silver powder and aluminum powder. With the help of the local channel opened by glass etching SiNx / AlOx dielectric layer, the low-melting point silver-aluminum liquid phase diffuses with silicon to form silver-aluminum spikes, which form direct contact and conduction with the p+ emitter and the metal grid line body, greatly improving the contact resistance. It is the most critical material that dominates the conversion efficiency of the entire TOPCon cell. Compared with the traditional PERC conductive paste using pure silver, the solid content and viscosity tend to be higher, which is relatively unfavorable for the storage stability of the paste and the mass production yield and long-term printing on narrow line width screens.

[0004] Therefore, there is an urgent need to provide a silver-aluminum conductive paste that is evenly dispersed, has low viscosity, and is more suitable for narrow-diameter and small-opening printing screens, so as to improve the above-mentioned mass production problems and thereby improve the battery conversion efficiency. Summary of the invention

[0005] The main purpose of the present invention is to provide a silver-aluminum conductive paste for the front side of a crystalline silicon solar cell with a fine line and good ink permeability through a tunneling oxide passivation contact, so as to solve the mass production problem of the conductive paste in the prior art, which has low cell conversion efficiency due to poor mesh permeability.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A front silver-aluminum paste for TOPCon solar cells, comprising 80-95wt% of conductive powder, 0.1-7wt% of glass powder and 1.5-15wt% of an organic vehicle paste composition, wherein the organic vehicle paste composition comprises a compounded resin, a compounded dispersant, an organic solvent and an additive. The content of the compounded resin in the conductive paste is 0.2-5wt%, and the content of the compounded dispersant in the conductive paste is 0.01-2wt%.

[0008] The composite resin comprises at least two of cellulose acetate, cellulose acetate butyrate, ethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polymethyl acrylate, polyethyl acrylate, polybutyl acrylate, polyisobutyl acrylate, styrene-acrylate copolymer, acrylonitrile-styrene-acrylate copolymer, hydrogenated styrene-isoprene copolymer, styrene-butadiene-styrene copolymer and styrene-[ethylene-(ethylene-propylene)]-styrene copolymer.

[0009] Preferably, the composite resin is selected from at least two of cellulose acetate, cellulose acetate butyrate, ethyl cellulose, polybutyl acrylate, styrene-acrylate copolymer, hydrogenated styrene-isoprene copolymer or styrene-butadiene-styrene copolymer.

[0010] First, the compounded resin can be used to more completely coat conductive powders such as silver powder and aluminum powder, which is beneficial to the grinding and dispersion effect in the subsequent slurry process, reduces the proportion of silver flakes, and helps the high-solid content conductive slurry to have good ink-passing properties. The compounded resin has a cohesive effect on the silver-aluminum conductive slurry, which can prevent the powder from collapsing or flowing significantly under high-temperature sintering, maintain the height morphology of the grid line, and thus effectively control the thinning ability of the secondary grid. The compounded resin also has an adhesive effect, which can respond to the different velvet polishing degrees on the silicon wafer, avoid the grid line from falling off due to the rapid shrinkage of the organic carrier and the volatilization of the solvent during high-temperature drying and sintering, and further improve the bonding strength between the slurry and the substrate.

[0011] The compound dispersant comprises at least two of TDO, oleic acid, ED120, ED350, ED420, isomeric decanol polyoxyethylene ether, isomeric undecanol polyoxyethylene ether and isomeric tridecanol polyoxyethylene ether.

[0012] Compound dispersants can promote better dispersion of inorganic powder in conductive paste, balance the performance of various components in the paste, avoid powder agglomeration, and achieve the lowest viscosity under high solid content paste formula design to meet the mass production process requirements of screen printing. Especially, compared with other combinations of resins and dispersants.

[0013] The organic solvent accounts for 1 to 10 wt % of the conductive paste. Preferably, the organic solvent is selected from the group consisting of ethyl cellosolve, butyl cellosolve, diethylene glycol monobutyl ether, diethylene glycol dibutyl ether, monobutyl ether acetate, propylene glycol monomethyl ether, diethylene glycol butyl ether acetate, alcohol ester dodeca, tripropylene glycol monomethyl ether, triacetin, triethylene glycol dibenzoate and terpineol.

[0014] The additives include thixotropic agents and plasticizers accounting for 0.5-5wt% of the conductive paste. Preferably, the additives are selected from one or more of the group consisting of polyvinyl butyral, polyurethane polyamide, polyamide, polydimethylsiloxane, polymethylphenylsiloxane, polyether polysiloxane copolymer, aminosiloxane and fumed silica.

[0015] Furthermore, the conductive powder comprises at least one conductive inorganic powder; preferably, the inorganic powder is silver powder and aluminum powder, the average particle size D50 of the silver powder is 0.1-5 μm, and the average particle size D50 of the aluminum powder is 0.3-8 μm.

[0016] Preferably, the glass powder is a glass powder based on lead oxide-tellurium oxide-bismuth oxide-zinc oxide; the glass powder also contains one or more selected from the group consisting of lithium oxide, sodium oxide, potassium oxide, magnesium oxide, calcium oxide, strontium oxide, barium oxide, phosphorus oxide, zinc oxide, silicon dioxide, boron oxide, titanium oxide and nickel oxide; preferably, the particle size (D50) of the glass powder is 1.5 to 2.0 μm.

[0017] Further, the silver-aluminum conductive paste comprises 83-93.5wt% of conductive powder, 0.8-4.5wt% of glass powder, 2-8.5wt% of organic solvent, 1-4.5wt% of additive, 0.4-3.5wt% of resin and 0.05-1.2wt% of dispersant, wherein the resin is composed of cellulose acetate butyrate, ethyl cellulose and styrene-acrylate copolymer; preferably, in the composition of the resin, the weight ratio of cellulose acetate butyrate, ethyl cellulose and styrene-acrylate copolymer is (1-2):(1-2.5):(4-8); wherein the dispersant is TDO and oleic acid; preferably, the weight ratio of TDO and oleic acid is (1-1.5):(1-2);

[0018] Further, the silver-aluminum conductive paste comprises 84.7-92.6wt% of conductive powder, 1.3-4wt% of glass powder, 2.7-9wt% of organic solvent, 2-4wt% of additive, 0.7-3wt% of compound resin and 0.05-1.6wt% of compound dispersant, wherein the resin is composed of cellulose acetate, polybutyl acrylate and styrene-acrylate copolymer; preferably, in the composition of the resin, the weight ratio of cellulose acetate, polybutyl acrylate and styrene-acrylate copolymer is (1-1.6):(1-2.3):(3-5.5); wherein the dispersant is ED350 and isomeric decanol polyoxyethylene ether; preferably, in the dispersant, the weight ratio of ED350 and isomeric decanol polyoxyethylene ether is (1-1.35):(1-1.6);

[0019] Further, the silver-aluminum conductive paste comprises 87-94wt% of conductive powder, 2.5-5wt% of glass powder, 3.5-9.3wt% of organic solvent, 2.5-4.2wt% of additives, 0.45-2.8wt% of compound resin and 0.1-1.3wt% of compound dispersant, wherein the resin is composed of polybutyl acrylate, styrene-acrylate copolymer or styrene-butadiene-styrene copolymer; preferably, in the composition of the resin, the weight ratio of polybutyl acrylate, styrene-acrylate copolymer or styrene-butadiene-styrene copolymer is (1-2):(1-3):(2-4); wherein the dispersant is oleic acid and isotridecyl alcohol polyoxyethylene ether; preferably, in the dispersant, the weight ratio of oleic acid and isotridecyl alcohol polyoxyethylene ether is (1-1.4):(1-2.5);

[0020] Furthermore, the silver-aluminum conductive paste comprises 85-94.7wt% of conductive powder, 3.5-6wt% of glass powder, 2.5-8.6wt% of organic solvent, 2-4.5wt% of additives, 0.5-2.9wt% of compound resin and 0.2-1wt% of compound dispersant, wherein the resin is composed of polybutyl acrylate, styrene-acrylate copolymer and hydrogenated styrene-isoprene copolymer; preferably, in the composition of the resin, the weight ratio of polybutyl acrylate, styrene-acrylate copolymer and hydrogenated styrene-isoprene copolymer is (1-3.4):(1-2.2):(3-5.5); wherein the dispersant is TDO and isomeric undecyl alcohol polyoxyethylene ether; preferably, in the dispersant, the weight ratio of TDO and isomeric undecyl alcohol polyoxyethylene ether is (1-1.8):(1-2).

[0021] The silver-aluminum conductive paste of the present invention is widely applicable when applied to screen printing, and can be applied to mesh counts of 480 / 500 / 520, wire diameters of 9 to 11um, yarn thicknesses of 12.5 to 15um, film thicknesses of 3.5 to 7um, and screen openings of 11 to 18μm. In addition, within this opening range, the requirements for thinning can be maintained while taking into account better ink passing capabilities. According to one aspect of the present invention, a solar cell electrode is provided, which is prepared from the silver-aluminum conductive paste, and preferably, the width of the solar cell electrode is 15 to 35μm.

[0022] The beneficial effects achieved by the present invention are: the present invention uses a specific type of resin carrier and dispersant combination to form a better match with other components such as conductive powder, and the components have a better synergistic effect as a whole, and will not bring any negative effects on the subsequent electrode production or application under high temperature sintering in solar cells, such as electrode conductivity, electrode aspect ratio and battery conversion efficiency. Furthermore, such a combination of resin and dispersant can effectively reduce the viscosity of the slurry with a high solid content, thereby improving the processing performance of the slurry in the subsequent printing process, such as: improving the ink-passing performance of the slurry, having better ink penetration ability, thereby promoting lower electrode resistance, avoiding the phenomenon of grid line breaking in electrode production or uneven ink return caused by adhesion to processing devices such as printing scrapers, and thus improving battery conversion efficiency. Most importantly, the above-mentioned conductive slurry has a relatively wide printing operation window, which is more suitable for advanced narrow line width opening printing screen operation, obtaining a finer line electrode, reducing the light-receiving area of ​​the silicon wafer, and improving the generation of photocurrent, thereby obtaining a higher battery conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0024] Figure 1 It is one of the schematic diagrams of the preparation process of the present invention;

[0025] Figure 2 It is one of the schematic diagrams of the preparation process of the present invention;

[0026] Figure 3 It is one of the schematic diagrams of the preparation process of the present invention;

[0027] Figure 4 It is one of the schematic diagrams of the preparation process of the present invention;

[0028] Figure 5 It is one of the schematic diagrams of the preparation process of the present invention;

[0029] Figure 6 It is one of the schematic diagrams of the preparation process of the present invention;

[0030] Figure 7 It is one of the schematic diagrams of the preparation process of the present invention;

[0031] Figure 8 It is one of the schematic diagrams of the preparation process of the present invention;

[0032] Fig. 9 It is one of the schematic diagrams of the preparation process of the present invention;

[0033] Among them, 10, N-type silicon substrate; 20, P layer; 30, front passivation layer; 40, back passivation layer; 50, back main grid silver electrode (after high-temperature sintering); 60, back auxiliary grid silver electrode (after high-temperature sintering); 70, front main grid silver electrode (after high-temperature sintering); 80, front auxiliary grid silver electrode (after high-temperature sintering). DETAILED DESCRIPTION

[0034] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0035] Example

[0036] An implementation example of a method for manufacturing an N-type silicon-based solar cell is shown below. However, the present invention is not limited to the following implementation example.

[0037] Figure 1 An N-type silicon substrate 10 is shown.

[0038] Figure 2 It is shown that the P layer 20 with reverse conductivity is formed by the thermal diffusion of boron (generally using boron tribromide BBr3 as the boron diffusion source). The crystalline silicon substrate is composed of an N-type silicon substrate 10 and a P layer 20 to form a PN junction.

[0039] Use an anti-corrosion agent to protect the surface of the P layer 20, remove the surrounding and bottom layers of the P layer 20 by etching, and only retain the main surface. Then use an organic solvent to remove the excess anti-corrosion agent, such as Figure 3 shown.

[0040] like Figure 4 As shown, a passivation layer 30 is formed on the P layer 20 using Al2O3 and SiNx as passivation layer materials through plasma chemical vapor deposition (PECVD), and a passivation layer 40 is formed on the back side of the N layer 10 using SiNx as passivation layer material.

[0041] like Figure 5 As shown, the back main grid silver paste 50 is printed onto the passivation layer 40 by screen printing and then dried.

[0042] like Figure 6As shown, the back side sub-gate silver paste 60 is printed onto the passivation layer 40 by screen printing and then dried.

[0043] like Figure 7 As shown, the front main grid silver paste 70 is printed onto the passivation layer 30 by screen printing and then dried.

[0044] like Figure 8 As shown, the front sub-gate silver aluminum paste 80 is printed onto the passivation layer 30 by screen printing and dried in sequence. Then, it is sintered in an infrared heating furnace at a peak temperature ranging from 400 to 950° C. Under different belt speeds of the sintering equipment, the total sintering time from entering to leaving the heating furnace is 30 seconds to 5 minutes, provided that the N-type silicon substrate 10 is prevented from having the defect of over-sintering and warping.

[0045] like Fig. 9 As shown, the dried back silver paste after high temperature sintering forms a back silver main grid electrode 50 and a back silver sub-grid 60, and the front part forms a front silver main grid electrode 70 and a back silver sub-grid 80. Through high temperature sintering, a good ohmic contact is formed at the front silver aluminum / silicon interface and the back silver / silicon interface to achieve electrical connection.

[0046] The front silver-aluminum conductive silver paste in the present invention can realize the expected narrow line width of the front silver-aluminum electrode through advanced screen printing screen design. With different screen opening designs, the electrode width after sintering in different embodiments is 17 to 30 um.

[0047] The present invention takes N-type silicon-based solar cells as an example, but is not limited thereto and may also be applicable to P-type silicon-based solar cells, back-contact solar cells, or other solar cell technologies formed using conductive pastes.

[0048] The present invention also provides a solar cell, comprising an electrode, wherein the electrode is the solar cell electrode as described above.

[0049] Based on the above reasons, the battery of the present invention has a better battery conversion rate.

[0050] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0051] The conductive pastes in the embodiments and comparative examples are made of the following materials.

[0052] Conductive powder: spherical silver powder, particle size (D50) is 1.2-2.1μm. The particle size D50 of aluminum powder is 0.3-8μm. The brand of silver powder is Japan DOWA4-8FD, and the brand of aluminum powder is ToyalTFH-A02P.

[0053] Glass powder: glass powder based on lead oxide-tellurium oxide-bismuth oxide-zinc oxide. Particle size (D50) is 1.5-2.0 μm, brand name BASS T2.

[0054] Resins: Including Eastman TM Cellulose acetate butyrate, ethyl cellulose, hydroxyethyl cellulose; polyethyl acrylate and polybutyl acrylate of Shanghai MacLean Biochemical Technology Co., Ltd.; synthetic latex AT-928 styrene-acrylate copolymer of Andes; at least two of styrene-butadiene-styrene copolymer of Taiwan Rubber Co., Ltd.

[0055] Dispersant: Included TDO; oleic acid from Shanghai Yuanji Chemical Co., Ltd. and two types of isomeric undecanol polyoxyethylene ether and isomeric tridecanol polyoxyethylene ether provided by BASF.

[0056] The brand of thixotropic agent is Nanben 6500. The brand of plasticizer is Dow Corning 200 Fluid 50 cSt.

[0057] The amounts of the above ingredients added are shown in Table 1.

[0058] The conductive paste is prepared by the following method: an organic solvent, a resin, an additive and a dispersant are mixed and stirred at 50 to 60°C with high shear force for 1 to 2 hours. Glass powder, silver powder and aluminum powder are added to the above mixture, and the paste composition is repeatedly rolled with a three-roll mill to grind the conductive paste to a fineness (FOG) of 15 / 10 μm or less.

[0059] Performance characterization:

[0060] (1) Viscosity test

[0061] 13-5 g of the slurry was sampled and the slurry viscosity value was presented using a Brookfield DV1 viscosity tester and a rotor SC-14 under the measurement conditions of 25°C / 50 rpm / 30 seconds.

[0062] (2) Electrode width and printability test

[0063] The conductive paste in the above embodiments and comparative examples is printed onto the SiN layer of the silicon wafer substrate (182×182mm) by screen printing technology. The electrical properties (electrode printing screen for testing battery conversion efficiency) and printing screen specifications used are respectively 500 mesh without mesh / 9μm wire diameter / total thickness 18-18.5μm / opening 13μm (narrow opening) and 500 mesh without mesh / 9μm wire diameter / total thickness 18-18.5μm / opening 16μm, 14μm, 12, 10μm (narrow opening). The battery cell is dried in an infrared drying furnace and then sintered in a belt sintering furnace at 920-930°C for 40 seconds. The sintered conductive paste is cooled to form an electrode. The width of the electrode is measured using an optical microscope and a micro-imaging inspection instrument. The resistance values ​​at different screen openings (16μm, 14μm, 12, 10μm) are directly measured by a resistance tester.

[0064] The ink passing performance (printability test) of the slurry under different screen openings is expressed by resistance value. The higher the resistance, the worse the ink passing ability.

[0065] (3) Battery conversion efficiency test

[0066] The formed solar cell is placed in a Berger solar cell tester under a light source condition for efficiency measurement. The xenon arc lamp in the solar cell tester simulates sunlight with a known intensity and radiates it on the light-receiving front surface of the cell. The voltage (V) and current (I) are measured under a load resistance setting of approximately 400 using a four-point contact method to determine the voltage-current curve of the cell, and the cell conversion efficiency (EFF) is calculated based on this curve.

[0067] Table 1

[0068]

[0069]

[0070] Table 1

[0071]

[0072]

[0073] Table 1

[0074]

[0075]

[0076] The difference between Examples 1 to 6 is that when the ratio of other raw materials is fixed, when comparing the additive combination with the addition amount of 0.55%, Examples 3, 4, and 5 all have lower slurry viscosity at 50rpm and lower resistance values ​​at different line width openings, which respectively use TDO / isotridecyl alcohol polyoxyethylene ether, oleic acid / isoundecyl alcohol polyoxyethylene ether, and oleic acid / isotridecyl alcohol polyoxyethylene ether. These three dispersant combinations are subsequently selected to further adjust the addition ratio of other raw materials.

[0077] The main difference between Examples 7 and 8 and Example 3 is the increase in the amount of silver powder. Accordingly, Example 7 increases the silver powder by 0.25wt%, reduces the additive by 0.15wt% and the solvent by 0.1%; Example 8 increases the silver powder by 0.5wt%, reduces the additive by 0.2wt% and the solvent by 0.3%.

[0078] The main difference between Examples 9 and 10 and Example 4 is the increase in the amount of silver powder. Accordingly, Example 9 increases the silver powder by 0.25wt%, reduces the additive by 0.15wt% and the solvent by 0.1%; Example 10 increases the silver powder by 0.5wt%, reduces the additive by 0.2wt% and the solvent by 0.3%.

[0079] The main difference between Examples 11 and 12 and Example 5 is the increase in the amount of silver powder. Accordingly, Example 11 increases the silver powder by 0.25wt%, reduces the additive by 0.15wt% and the solvent by 0.1%; Example 12 increases the silver powder by 0.5wt%, reduces the additive by 0.2wt% and the solvent by 0.3%.

[0080] The above adjustment of increasing the silver content by 0.25-0.5wt%, using TDO / isomeric tridecanol polyoxyethylene ether, Examples 7 and 8 obtained higher viscosity and resistivity, but did not reflect the improvement in efficiency. Using oleic acid / isomeric undecanol polyoxyethylene ether, Examples 9 and 10 also obtained an increase in viscosity, which was reflected in a reasonable increase in resistivity, and also obtained an increase in efficiency of 0.08-0.09%. Using oleic acid / isomeric tridecanol polyoxyethylene ether, Examples 11 and 12 were also reflected in the increase in viscosity and resistivity, but the efficiency gain was not obvious. The above results show that oleic acid / isomeric undecanol polyoxyethylene ether can provide the widest printing window, with less viscosity increase, narrow electrode width and the best printability resistance value performance, which can be further matched with the adjustment of organic carriers or inorganic powders to provide efficiency gains and find the critical value of raw material addition.

[0081] The main difference between Examples 13 and 14 and Example 4 is that the amount of silver powder is further increased. Accordingly, Example 13 increases 0.75wt% of silver powder, reduces 0.25wt% of additives and 0.5% of solvents; Example 14 increases 1wt% of silver powder, reduces 0.3wt% of additives and 0.7% of solvents. Example 13 with 0.75wt% of silver powder has further efficiency gains compared to Examples 4, 9, and 10, and the viscosity and line resistivity are still within the controllable range. Compared with Example 14 with 1wt% of silver powder, the overall viscosity and line resistivity have exceeded the theoretical standard, and there is no efficiency gain, which is already within the adjustment range of the outlier value.

[0082] The main difference between Examples 15 and 16 and Example 10 is the adjustment of the ratio of the resin cellulose acetate butyrate and the styrene-butadiene-styrene copolymer. Accordingly, Example 15 reduces 0.15wt% of cellulose acetate butyrate and increases 0.15wt% of styrene-butadiene-styrene copolymer; Example 16 increases 0.15wt% of cellulose acetate butyrate and reduces 0.15wt% of styrene-butadiene-styrene copolymer. Example 15, which reduces the high-polarity resin cellulose acetate butyrate and increases the low-polarity resin styrene-butadiene-styrene copolymer, can reduce the overall slurry viscosity, further improve the efficiency by 0.03% and have a lower line resistivity. On the contrary, Example 16, which increases the high-polarity resin cellulose acetate butyrate and reduces the low-polarity resin styrene-butadiene-styrene copolymer, has a slightly worse printability due to the higher viscosity, increased line resistivity, and the overall grid line height decreases instead of increases, thus having no efficiency advantage.

[0083] In Examples 17 and 18, the proportion and ratio of the dispersant composition are further adjusted based on the advantages of increasing the silver content in Example 13 and reducing the high-polarity resin cellulose acetate butyrate in Example 15, and increasing the low-polarity resin styrene-butadiene-styrene copolymer. Accordingly, Example 17 fixes the total amount of dispersant at 0.55wt%, increases the proportion of oleic acid to be higher than isomeric undecyl alcohol polyoxyethylene ether; Example 18 fixes the proportion of oleic acid and isomeric undecyl alcohol polyoxyethylene ether, and reduces the overall addition amount by 0.25wt%. Both Example 17, which increases the proportion of dispersant oleic acid, and Example 18, which fixes the proportion of dispersant and reduces the addition amount, can provide lower viscosity and lower line resistance than Example 13 at the same silver content, and better ink permeability also further contributes to a slight increase in efficiency, and has better adaptability to mass production.

[0084] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A front silver-aluminum paste for TOPCon solar cells, characterized in that: Containing 80-95wt% of conductive powder, 0.1-7wt% of glass powder and 1.5-15wt% of organic vehicle paste composition; The organic carrier paste composition comprises a compound resin, a compound dispersant, an organic solvent and an additive; the proportions of each component in the front silver-aluminum paste are: 0.2-5wt% of the compound resin, 0.01-2wt% of the compound dispersant, 1-10wt% of the organic solvent, and 0.5-5wt% of the additive; The compound resin is a mixture of cellulose acetate butyrate, polybutyl acrylate, and styrene-butadiene-styrene copolymer; the mass ratio of cellulose acetate butyrate: polybutyl acrylate: styrene-butadiene-styrene copolymer is 0.3:0.2:1.0; The compound dispersant is at least two of TDO, oleic acid, isomeric undecanol polyoxyethylene ether and isomeric tridecanol polyoxyethylene ether.

2. The front silver-aluminum paste for TOPCon solar cells according to claim 1, characterized in that: The organic solvent is selected from one or more of the group consisting of ethyl cellosolve, butyl cellosolve, diethylene glycol monobutyl ether, diethylene glycol dibutyl ether, monobutyl ether acetate, propylene glycol monomethyl ether, diethylene glycol butyl ether acetate, alcohol ester dodecahydrate, tripropylene glycol monomethyl ether, triacetin, triethylene glycol dibenzoate and terpineol.

3. The front silver-aluminum paste for TOPCon solar cells according to claim 1, characterized in that: The additive is one or more selected from the group consisting of polyvinyl butyral, polyurethane polyamide, polyamide, polydimethylsiloxane, polymethylphenylsiloxane, polyether polysiloxane copolymer, aminosiloxane and fumed silica.

4. The front silver-aluminum paste for TOPCon solar cells according to claim 1, characterized in that: The conductive powder is composed of silver powder and aluminum powder. The average particle size D50 of the silver powder is 0.1-5 μm, and the average particle size D50 of the aluminum powder is 0.3-8 μm.

5. The front silver-aluminum paste for TOPCon solar cells according to claim 1, characterized in that: The glass powder is a glass powder based on lead oxide-tellurium oxide-bismuth oxide-zinc oxide, and also contains one or more selected from the group consisting of lithium oxide, sodium oxide, potassium oxide, magnesium oxide, barium oxide, phosphorus oxide, silicon dioxide, boron oxide, titanium oxide and nickel oxide. The particle size D50 of the glass powder is 1.5 to 2.0 μm.

6. Use of the front silver-aluminum paste for TOPCon solar cells according to any one of claims 1 to 5 in the preparation of solar cells.

7. A solar cell electrode, characterized in that: The solar cell electrode is prepared from the front silver-aluminum paste for TOPCon solar cells according to any one of claims 1 to 5, wherein the width of the solar cell electrode is 15 to 35 μm.

Citation Information

Patent Citations

  • Conductive paste and application thereof, solar cell electrode and solar cell

    CN109903885A

  • Conductive slurry, preparation method and application of conductive slurry, solar cell electrode containing conductive slurry and solar cell

    CN110504070A