A method for preparing N-type tellurene based on iodine vapor doping method
The two-dimensional tellurene N-type doping method is solved by iodine steam doping, which solves the problem of maturity and stability of the two-dimensional material doping process, and realizes efficient and simple preparation of N-type tellurene field effect transistors, which is suitable for low-energy Circuit consumption application.
Patent Information
- Application Number
- CN202311257435.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-09-27
AI Technical Summary
The doping process of two-dimensional materials is not mature enough, and it is difficult to accurately control the carrier concentration and stability, which affects the application of two-dimensional materials in low-energy-consuming circuits.
The two-dimensional tellurylene is N-type doped by using the iodine steam doping method. By heating the solid iodine to 30°C to 45°C in a closed cavity, it is sublimated into iodine vapor for 4-9 hours. A N-type tellurylene field effect transistor is formed.
A simple, controllable, safe and pollution-free doping process is realized, and an efficient N-type telluryl field effect transistor is prepared, with the characteristics of good repeatability, low cost and suitable for industrial production.
Smart Images

Figure CN116994943B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of field effect transistor modification of semiconductor devices, and in particular to a method for preparing an N-type tellurene field effect transistor based on an iodine vapor doping method. Background Art
[0002] Two-dimensional materials have great application potential in the fields of electronics, optoelectronics and sensing. However, compared with traditional silicon process production lines, two-dimensional materials still have a long way to go. For example, the doping process of two-dimensional materials is not mature enough. The emergence of new two-dimensional materials poses a huge challenge to the precise and long-term stable control of "effective doping". Ideally, it is necessary to determine appropriate parameters to replace two-dimensional crystal atoms and to be able to effectively and accurately control the carrier concentration in order to efficiently implement control in later low-energy circuits. The doping process of two-dimensional materials is not only a requirement for channel materials in the future electronics industry, but also a necessary experimental process to obtain the physical and chemical properties of two-dimensional materials.
[0003] Compared with traditional silicon, atomically thin tellurene has the following advantages in the application of field effect transistor channel materials: higher mobility; relatively high current switching; very stable in air. However, there is still a lack of an efficient and simple method for doping atomically thin tellurene. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention discloses a method for preparing an N-type tellurene field effect transistor based on an iodine vapor doping method.
[0005] According to a first aspect of an embodiment of the present invention, a method for preparing N-type tellurene based on an iodine vapor doping method is provided, the preparation method comprising:
[0006] Providing two-dimensional tellurene;
[0007] Two-dimensional tellurene is placed in a closed cavity and doped with iodine vapor to obtain N-type tellurene.
[0008] Further, doping the two-dimensional tellurene with iodine vapor includes: heating solid iodine to 30° C. to 45° C. to sublimate the solid iodine into iodine vapor for 4 to 9 hours. Preferably, heating the solid iodine to 30° C. to sublimate the solid iodine into iodine vapor for 5 hours.
[0009] According to a second aspect of an embodiment of the present invention, there is provided an N-type tellurene, which is prepared by the above-mentioned method for preparing N-type tellurene based on the iodine vapor doping method.
[0010] According to a third aspect of an embodiment of the present invention, there is provided a method for preparing an N-type tellurene field effect transistor based on an iodine vapor doping method, the method comprising:
[0011] Providing two-dimensional tellurene;
[0012] Placing two-dimensional tellurene on a silicon / silicon dioxide substrate with a back electrode to obtain a first sample;
[0013] Prepare a source electrode and a drain electrode at two ends of the first sample;
[0014] The first sample is placed upside down in a sealed cavity, and the two-dimensional tellurene is doped with iodine vapor to obtain a gate dielectric layer.
[0015] Furthermore, gold / palladium electrodes are selected as the source and drain electrodes.
[0016] Further, doping the two-dimensional tellurene with iodine vapor includes: heating solid iodine to 30° C. to 45° C. to sublimate the solid iodine into iodine vapor for 4 to 9 hours. Preferably, heating the solid iodine to 30° C. to sublimate the solid iodine into iodine vapor for 5 hours.
[0017] According to a fourth aspect of an embodiment of the present invention, there is provided an N-type tellurene field effect transistor, comprising the above-mentioned N-type tellurene or the above-mentioned method for preparing the N-type tellurene field effect transistor based on iodine vapor doping method.
[0018] According to a fifth aspect of an embodiment of the present invention, a chip is provided, comprising a chip body and the N-type tellurene field effect transistor as described above, wherein the N-type tellurene field effect transistor is arranged on the chip body.
[0019] According to a sixth aspect of an embodiment of the present invention, there is provided a circuit, comprising a circuit board main body and the above-mentioned chip, wherein the chip is arranged on the circuit board main body.
[0020] According to a seventh aspect of an embodiment of the present invention, there is provided a device, comprising a housing and the above-mentioned circuit, wherein the circuit is arranged on the housing.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The present invention doped two-dimensional tellurene with iodine vapor to convert the originally P-type two-dimensional tellurene into N-type tellurene, and prepared an N-type tellurene field effect transistor based on the N-type tellurene.
[0023] (2) The present invention has conducted a detailed study on the doping process of iodine vapor and found an efficient doping parameter of iodine vapor by adjusting its thermodynamic process.
[0024] (3) The process of the present invention is simple and controllable, with a short preparation cycle, safe, pollution-free and low-cost. According to actual production requirements, materials or devices can be doped flexibly, and no obvious impurities are generated after doping. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.
[0026] Figure 1 A flow chart of a method for preparing N-type tellurene based on iodine vapor doping method provided in an embodiment of the present invention;
[0027] Figure 2 A microscope photo of two-dimensional tellurene provided in an embodiment of the present invention;
[0028] Figure 3 Microscope photos of two-dimensional tellurene before and after doping provided by an embodiment of the present invention;
[0029] Figure 4 A scanning electron microscope image of N-type tellurene provided in an embodiment of the present invention;
[0030] Figure 5 A flow chart of a method for preparing an N-type tellurene field effect transistor based on an iodine vapor doping method provided in an embodiment of the present invention;
[0031] Figure 6 A schematic diagram of a closed cavity provided by an embodiment of the present invention;
[0032] Figure 7 A scanning electron microscope image of an N-type tellurene field effect transistor provided by an embodiment of the present invention;
[0033] Figure 8 A microscope photograph of an N-type tellurene field effect transistor provided in an embodiment of the present invention;
[0034] Fig. 9 is a transfer characteristic curve diagram of the N-type tellurene field effect transistor obtained in Example 1 of the present invention;
[0035] Fig.10 The transfer characteristic curve diagram corresponding to the product obtained in Example 2 of the present invention;
[0036] Fig.11 The transfer characteristic curve diagram corresponding to the product obtained in Example 3 of the present invention;
[0037] Fig.12 The transfer characteristic curve diagram corresponding to the product obtained in Example 4 of the present invention;
[0038] Fig.13 This is a transfer characteristic curve diagram corresponding to the product obtained in Example 6 of the present invention. DETAILED DESCRIPTION
[0039] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are merely examples of devices and methods consistent with some aspects of the present invention as detailed in the appended claims.
[0040] The terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The singular forms "a", "the" and "the" used in the present invention and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.
[0041] It should be understood that although the terms first, second, third, etc. may be used in the present invention to describe various information, these information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of the present invention, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Depending on the context, the word "if" as used herein may be interpreted as "at the time of" or "when" or "in response to determining".
[0042] The purpose of the present invention is to provide a method for preparing N-type tellurene based on iodine vapor doping method, which successfully dopes tellurene that was originally a narrow bandgap P-type to form an N-type semiconductor. The method is simple and is carried out at a relatively low temperature without any impact on the device itself. This process has good repeatability and has the potential to be an important means for mass production of tellurene field effect transistors in the future. The N-type tellurene prepared by this method can be used as a gate in an effect transistor to effectively control the source-drain current. The method utilizes the chemical activity of tellurene itself to form an oxide film on the tellurium surface to form a dense gate dielectric. The method has good repeatability and low cost, and is easy to mass produce tellurene field effect transistor gate dielectrics in the industry in the future.
[0043] The present invention is described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the features of the following embodiments and implementations can be combined with each other.
[0044] like Figure 1 As shown, the present invention provides a method for preparing N-type tellurene based on iodine vapor doping method, and the method specifically comprises the following steps:
[0045] S100, providing two-dimensional tellurene.
[0046] In the embodiments of the present invention, two-dimensional tellurene is prepared by following the steps in "Wang Yixiu, Qiu Gang, Wang Ruoxing, et al. Field-effect transistors made from solution-grown two-dimensional tellurene[J]. Nature Electronics, 2018, 1(4): 228-236. doi: 10.1038 / s41928-018-0058-4". The steps include:
[0047] 0.1 g of sodium tellurite and 0.5 g of polyvinyl pyrrolidone with a molecular weight of 58,000 were dissolved in 33 mL of deionized water with a conductivity of 18.2 MΩ•cm, and stirred for 30 minutes under a magnetic stirrer to form a solution A with a concentration of 0.014 mol / L. Subsequently, 1.65 mL of hydrazine hydrate and 3.3 mL of ammonia water were mixed to form a solution B, which was added to the solution A and placed in a hydrothermal reaction vessel. After sealing, the solution was reacted in an oven at 160°C for 30 hours and then taken out to obtain the product two-dimensional tellurene. The microscope photo of the two-dimensional tellurene is shown in FIG. Figure 2 As shown, the product two-dimensional tellurene was transferred to a 100nm SiO2 / Si P++ substrate after repeated washing with acetone and isopropanol for several times.
[0048] Furthermore, the hydrothermal reaction container is a reaction kettle, an electric pressure cooker, a soup pot or a beaker.
[0049] S110, placing the two-dimensional tellurene in a closed cavity, and doping the two-dimensional tellurene with iodine vapor to obtain N-type tellurene. Figure 3 As shown, Figure 3 a in the figure is the narrow bandgap P-type two-dimensional tellurene before doping. Figure 3 The b in the figure is N-type tellurene obtained by doping.
[0050] Wherein, doping the two-dimensional tellurene with iodine vapor includes: heating solid iodine to 30° C. to 45° C. to sublimate the solid iodine into iodine vapor for 4 to 9 hours. Preferably, heating the solid iodine to 30° C. to sublimate the solid iodine into iodine vapor for 5 hours.
[0051] The embodiment of the present invention further provides an N-type tellurene, which is prepared by the above-mentioned method for preparing N-type tellurene based on iodine vapor doping method. The method of the present invention successfully dopes tellurene, which is originally a narrow bandgap P-type, into an N-type semiconductor.
[0052] It should be noted that in the process of placing two-dimensional tellurene into a closed cavity, solid iodine is placed at the bottom of the closed cavity, and the two-dimensional tellurene is placed at the top of the closed cavity. In particular, the side to be doped needs to face downward, so that the solid iodine sublimates into iodine vapor, and the iodine vapor contacts the side to be doped, thereby completing the doping of the two-dimensional tellurene.
[0053] Furthermore, the EDS mapping of the scanning electron microscope was used to characterize the element content. Figure 4 result. Figure 4 (A) is a picture of the obtained product under a scanning electron microscope (SEM). Figure 4 (B) in the graph represents the content of tellurium. Figure 4 The (C) in the equation represents the content of iodine. Figure 4 From the EDS mapping results, it can be seen that iodine is detected on the tellurene two-dimensional crystal, indicating that the iodine doping process is effective.
[0054] The embodiment of the present invention further provides an N-type tellurene, which is prepared by the above-mentioned preparation method of N-type tellurene based on iodine vapor doping method.
[0055] like Figure 5 As shown, an embodiment of the present invention provides a method for preparing an N-type tellurene field effect transistor based on an iodine vapor doping method, the method comprising:
[0056] Step S200, providing two-dimensional tellurene, and placing the two-dimensional tellurene on a silicon / silicon dioxide substrate to obtain a first sample.
[0057] In the embodiments of the present invention, two-dimensional tellurene is prepared by following the steps in "Wang Yixiu, Qiu Gang, Wang Ruoxing, et al. Field-effect transistors made from solution-grown two-dimensional tellurene[J]. Nature Electronics, 2018, 1(4): 228-236. doi: 10.1038 / s41928-018-0058-4". The steps include:
[0058] 0.1g sodium tellurite and 0.5g polyvinyl pyrrolidone with a molecular weight of 58000 were dissolved in 33mL deionized water with a conductivity of 18.2MΩ•cm, and stirred under a magnetic stirrer for 30 minutes to form a solution A with a concentration of 0.014mol / L. Subsequently, 1.65mL hydrazine hydrate and 3.3mL ammonia water were mixed to form a solution B, which was added to the solution A and placed in a hydrothermal reaction container. After sealing, the solution was reacted in an oven at 160°C for 30 hours and taken out to obtain a two-dimensional tellurene product with a synthetic width of about 15 microns and a thickness of only tens of nanometers. The product was repeatedly washed with acetone and isopropanol for many times, and the two-dimensional tellurene product was transferred to a 100nm SiO2 / SiP++ substrate.
[0059] Furthermore, the hydrothermal reaction container is a reaction kettle, an electric pressure cooker, a soup pot or a beaker.
[0060] Step S210, placing two-dimensional tellurene on a silicon / silicon dioxide substrate with a back electrode to obtain a first sample;
[0061] Step S220, preparing a source electrode and a drain electrode at both ends of the first sample to obtain a second sample;
[0062] Specifically, the source and drain electrodes are prepared at both ends of the first sample through a standard micro-nano processing flow (spinning-exposure-development-evaporation). In this example, gold / palladium electrodes are used as the source and drain electrodes.
[0063] Step S230, placing the second sample upside down in a sealed cavity, and doping the two-dimensional tellurene with iodine vapor to obtain a gate dielectric layer; wherein the doping of the two-dimensional tellurene with iodine vapor includes: heating solid iodine to 30° C. to 45° C. to sublimate the solid iodine into iodine vapor for 4-9 hours. Preferably, heating the solid iodine to 30° C. to sublimate the solid iodine into iodine vapor for 5 hours.
[0064] It should be noted that if Figure 6 As shown, in the process of placing two-dimensional tellurene into a closed cavity, solid iodine is placed at the bottom of the closed cavity, and the second sample is placed at the top of the closed cavity. In particular, the second sample is placed upside down in the closed cavity, with the side to be doped facing downward, so that the solid iodine sublimates into iodine vapor, and the iodine vapor contacts the side to be doped, completing the doping and obtaining an N-type tellurene field effect transistor.
[0065] It should be noted that, in this example, the steps of preparing the source and drain and iodine vapor doping can be interchanged, and there is no restriction on the order of precedence, that is, the two-dimensional tellurene can be doped with iodine vapor first, and then the source and drain can be processed.
[0066] In summary, the present invention aims at preparing high-performance tellurene field effect transistors, and uses iodine vapor to perform N-type doping on tellurium at a relatively low temperature. The method is simple and easy to repeat, and the doped field effect transistor exhibits N-type characteristics, which is an efficient preparation method. It has the characteristics of good repeatability, simple operation, low cost and ease of industrialization. It provides a new technical means for the large-scale application of tellurene in the chip field in the future.
[0067] An embodiment of the present invention further provides an N-type tellurene field effect transistor, comprising the above-mentioned N-type tellurene or prepared by the above-mentioned method for preparing the N-type tellurene field effect transistor based on the iodine vapor doping method.
[0068] Example 1
[0069] This embodiment 1 is a preferred embodiment, and the steps of preparing an N-type tellurene field effect transistor are as follows:
[0070] Step S1, providing two-dimensional tellurene, and placing the two-dimensional tellurene on a silicon / silicon dioxide substrate with a back electrode to obtain a first sample.
[0071] Step S2, inverting the clean first sample obtained in step S1 into a closed cavity, doping the two-dimensional tellurene with iodine vapor, heating the solid iodine to 30° C. to sublimate the solid iodine into iodine vapor for 5 hours, and obtaining a second sample.
[0072] Step S3, the second sample obtained in step S2 is processed through a standard micro-nano processing process (spinning-exposure-development-evaporation) to prepare a simple two-terminal device with two gold / palladium electrodes for source and drain. The scanning electron microscope image of the device is shown in FIG. Figure 7 As shown. A microscope photo of a tellurene field effect transistor with two-dimensional tellurene in the same row is shown Figure 8 shown.
[0073] Step S4, using a probe station and a semiconductor tester to perform a standard semiconductor test on the transfer characteristic curve of the field effect transistor, that is, to test the current voltage curve between the source and drain electrodes to obtain an IV curve. The transfer characteristic curve is as follows: Fig. 9 As shown. Fig. 9 The transfer characteristic curve of the two-dimensional tellurene clearly shows that it has the transfer characteristics of an N-type semiconductor. The transfer characteristics of the two-dimensional tellurene are originally P-type. Preferred Example 1 shows that the method of the present invention successfully transforms P-type tellurene into an N-type semiconductor by doping with iodine vapor.
[0074] Example 2
[0075] Step S1, providing two-dimensional tellurene, and placing the two-dimensional tellurene on a silicon / silicon dioxide substrate with a back electrode to obtain a first sample.
[0076] Step S2: Place the clean first sample obtained in step S1 upside down into a closed cavity, heat it to 30 degrees for 5 hours, and then take it out to obtain a second sample.
[0077] Step S3: The second sample in step S2 is processed through a standard micro-nano processing flow (spinning-exposure-development-evaporation) to prepare a simple two-terminal device with two gold / palladium electrodes for source and drain.
[0078] Step S4: Use a probe station and a semiconductor tester to perform a standard semiconductor test on the transfer characteristic curve of the field effect transistor. The transfer characteristic curve is as follows: Fig.10 shown.
[0079] In Example 2, the addition of iodine is removed, and its transfer characteristic curve is found to be P-type, which is the characteristic of P-type of tellurene itself. Therefore, it is proved that the present invention realizes N-type transformation by iodine doping, which is independent of heating temperature and time.
[0080] Example 3
[0081] Step S1, providing two-dimensional tellurene, and placing the two-dimensional tellurene on a silicon / silicon dioxide substrate with a back electrode to obtain a first sample.
[0082] Step S2: Invert the clean first sample obtained in step S1 and place it in a closed cavity, dope the two-dimensional tellurene with iodine vapor, place solid iodine in it and heat it to 30 degrees for 3 hours, then take it out to obtain a second sample.
[0083] Step S3: The second sample in step S2 is processed through a standard micro-nano processing flow (spinning-exposure-development-evaporation) to prepare a simple two-terminal device with two gold / palladium electrodes for source and drain.
[0084] Step S4: Use a probe station and a semiconductor tester to perform a standard semiconductor test on the transfer characteristic curve of the field effect transistor. The transfer characteristic curve is as follows: Fig.11 As shown in (A), the microscope photo of the device is shown in Fig.11 As shown in (B) in the figure.
[0085] In this embodiment 3, the doping time is reduced, and it is found that the doping effect is not ideal. Fig.11 It can be seen from the transfer characteristic curve that its carriers are partly vacancies and partly electrons, and the N-type transition has not been fully realized.
[0086] Example 4
[0087] Step S1, providing two-dimensional tellurene, and placing the two-dimensional tellurene on a silicon / silicon dioxide substrate with a back electrode to obtain a first sample.
[0088] Step S2: Invert the clean first sample obtained in step S1 and place it in a closed cavity, dope the two-dimensional tellurene with iodine vapor, place it in solid iodine and heat it to 30 degrees for 7 hours, then take it out to obtain a second sample.
[0089] Step S3: The second sample in step S2 is processed through a standard micro-nano processing flow (spinning-exposure-development-evaporation) to prepare a simple two-terminal device with two gold / palladium electrodes for source and drain.
[0090] Step S4: Use a probe station and a semiconductor tester to perform a standard semiconductor test on the transfer characteristic curve of the field effect transistor. The transfer characteristic curve is as follows: Fig.12 As shown in (A), the microscope photo of the device is shown in Fig.12 As shown in (B) in the figure.
[0091] Example 4: The iodine doping time is extended to 7 hours, and the transfer characteristic curve Fig.12 As shown, the field effect transistor becomes N-type again. This embodiment shows that after 5 hours, iodine vapor doping can achieve the effect of N-type.
[0092] Example 5
[0093] Step S1, providing two-dimensional tellurene, and placing the two-dimensional tellurene on a silicon / silicon dioxide substrate with a back electrode to obtain a first sample.
[0094] Step S2: Invert the clean first sample obtained in S1 and place it in a closed cavity, dope the two-dimensional tellurene with iodine vapor, place it in solid iodine and heat it to 30 degrees for 10 hours, then take it out to obtain a second sample.
[0095] Step S3: The second sample in S2 is processed through a standard micro-nano processing flow (spinning-exposure-development-evaporation) to prepare a simple two-terminal device with two gold / palladium electrodes for source and drain.
[0096] Step S4: Use a probe station and a semiconductor tester to perform a standard semiconductor test on the transfer characteristic curve of the field effect transistor.
[0097] In this embodiment 5, the doping time is further prolonged, but the source and drain of the field effect transistor are disconnected. This embodiment shows that the doping time should not be too long, otherwise it will affect the semiconductor properties of the channel material itself.
[0098] Example 6
[0099] Step S1, providing two-dimensional tellurene, and placing the two-dimensional tellurene on a silicon / silicon dioxide substrate with a back electrode to obtain a first sample.
[0100] Step S2: Place the clean first sample obtained in S1 upright in a closed cavity, dope the two-dimensional tellurene with iodine vapor, place solid iodine in it and heat it to 30 degrees for 7 hours, then take it out to obtain a second sample.
[0101] Step S3: The second sample in S2 is processed through a standard micro-nano processing flow (spinning-exposure-development-evaporation) to prepare a simple two-terminal device with two gold / palladium electrodes for source and drain.
[0102] Step S4: Use a probe station and a semiconductor tester to perform a standard semiconductor test on the transfer characteristic curve of the field effect transistor. The transfer characteristic curve is as follows: Fig.13 As shown in (A), the microscope photo of the device is shown in Fig.13 As shown in (B) in the figure.
[0103] In Example 6, the sample is placed upright for doping. Fig.13 It can be found that the field effect transistor still has P-type characteristics. Therefore, the effect of doping the upright sample is not good.
[0104] Example 7
[0105] Step S1: providing two-dimensional tellurene;
[0106] Step S2: placing two-dimensional tellurene in a closed cavity, and doping the two-dimensional tellurene with iodine vapor to obtain N-type tellurene; wherein, doping the two-dimensional tellurene with iodine vapor includes: heating solid iodine to 33° C. to sublimate the solid iodine into iodine vapor for 4 hours.
[0107] The element content of the product obtained in Example 7 was characterized by EDS mapping using a scanning electron microscope. It can be observed that iodine element was detected on the tellurene two-dimensional crystal, indicating that the iodine doping process in Example 7 was effective.
[0108] Example 8
[0109] Step S1: providing two-dimensional tellurene;
[0110] Step S2: placing two-dimensional tellurene in a closed cavity, and doping the two-dimensional tellurene with iodine vapor to obtain N-type tellurene; wherein, doping the two-dimensional tellurene with iodine vapor includes: heating solid iodine to 35° C. to sublimate the solid iodine into iodine vapor for 5 hours.
[0111] The element content of the product obtained in Example 8 was characterized by EDS mapping using a scanning electron microscope. It can be observed that iodine element was detected on the tellurene two-dimensional crystal, indicating that the iodine doping process in Example 8 was effective.
[0112] Example 9
[0113] Step S1: providing two-dimensional tellurene;
[0114] Step S2: placing the two-dimensional tellurene in a closed cavity, and doping the two-dimensional tellurene with iodine vapor to obtain N-type tellurene; wherein, doping the two-dimensional tellurene with iodine vapor includes: heating solid iodine to 38° C. to sublimate the solid iodine into iodine vapor for 4.5 hours.
[0115] The element content of the product obtained in Example 9 was characterized by EDS mapping using a scanning electron microscope. It can be observed that iodine element was detected on the tellurene two-dimensional crystal, indicating that the iodine doping process in Example 9 was effective.
[0116] Example 10
[0117] Step S1: providing two-dimensional tellurene;
[0118] Step S2: placing two-dimensional tellurene in a closed cavity, and doping the two-dimensional tellurene with iodine vapor to obtain N-type tellurene; wherein, doping the two-dimensional tellurene with iodine vapor includes: heating solid iodine to 40° C. to sublimate the solid iodine into iodine vapor for 6 hours.
[0119] The element content of the product obtained in Example 10 was characterized by EDS mapping using a scanning electron microscope. It can be observed that iodine element was detected on the tellurene two-dimensional crystal, indicating that the iodine doping process in Example 10 was effective.
[0120] Embodiment 11
[0121] Step S1: providing two-dimensional tellurene;
[0122] Step S2: placing two-dimensional tellurene in a closed cavity, and doping the two-dimensional tellurene with iodine vapor to obtain N-type tellurene; wherein, doping the two-dimensional tellurene with iodine vapor includes: heating solid iodine to 42° C. to sublimate the solid iodine into iodine vapor for 5 hours.
[0123] The element content of the product obtained in Example 11 was characterized by EDS mapping using a scanning electron microscope. It can be observed that iodine element was detected on the tellurene two-dimensional crystal, indicating that the iodine doping process in Example 11 was effective.
[0124] Example 12
[0125] Step S1: providing two-dimensional tellurene;
[0126] Step S2: placing two-dimensional tellurene in a closed cavity, and doping the two-dimensional tellurene with iodine vapor to obtain N-type tellurene; wherein, doping the two-dimensional tellurene with iodine vapor includes: heating solid iodine to 45° C. to sublimate the solid iodine into iodine vapor for 9 hours.
[0127] The element content of the product obtained in Example 12 was characterized by EDS mapping using a scanning electron microscope. It can be observed that iodine element was detected on the tellurene two-dimensional crystal, indicating that the iodine doping process in Example 12 was effective.
[0128] Embodiment 13
[0129] Step S1: providing two-dimensional tellurene;
[0130] Step S2: placing two-dimensional tellurene in a closed cavity, and doping the two-dimensional tellurene with iodine vapor to obtain N-type tellurene; wherein, doping the two-dimensional tellurene with iodine vapor includes: heating solid iodine to 45° C. to sublimate the solid iodine into iodine vapor for 5 hours.
[0131] The element content of the product obtained in Example 13 was characterized by EDS mapping using a scanning electron microscope. It can be observed that iodine element was detected on the tellurene two-dimensional crystal, indicating that the iodine doping process in Example 13 was effective.
[0132] Embodiment 14
[0133] Step S1, providing two-dimensional tellurene, and placing the two-dimensional tellurene on a silicon / silicon dioxide substrate with a back electrode to obtain a first sample.
[0134] Step S2, inverting the clean first sample obtained in step S1 into a closed cavity, doping the two-dimensional tellurene with iodine vapor, heating the solid iodine to 32° C. to sublimate the solid iodine into iodine vapor for 9 hours, and obtaining a second sample.
[0135] Step S3, preparing a simple two-terminal device with two gold / palladium electrodes for source and drain on the second sample.
[0136] Step S4, using a probe station and a semiconductor tester to perform a standard semiconductor test on the transfer characteristic curve of the two-terminal device. By observing the transfer characteristic curve, it can be seen that the device prepared in Example 14 exhibits N-type semiconductor characteristics, indicating that Example 14 successfully converts P-type tellurene into an N-type semiconductor by doping with iodine vapor.
[0137] Embodiment 15
[0138] Compared with Example 14, the only difference is that the two-dimensional tellurene is doped with iodine vapor, and the solid iodine is heated to 34° C. to sublimate the solid iodine into iodine vapor for 8 hours.
[0139] The transfer characteristic curve corresponding to the two-terminal device prepared in Example 15 is obtained. By observing the transfer characteristic curve, it can be seen that the device prepared in Example 15 exhibits N-type semiconductor characteristics, indicating that Example 15 successfully converts P-type tellurene into an N-type semiconductor through iodine vapor doping.
[0140] Example 16
[0141] Compared with Example 14, the only difference is that the two-dimensional tellurene is doped with iodine vapor, and the solid iodine is heated to 36° C. to sublimate the solid iodine into iodine vapor for 6 hours.
[0142] The transfer characteristic curve corresponding to the two-terminal device prepared in Example 16 is obtained. By observing the transfer characteristic curve, it can be seen that the device prepared in Example 16 exhibits N-type semiconductor characteristics, indicating that Example 16 successfully converts P-type tellurene into an N-type semiconductor through iodine vapor doping.
[0143] Embodiment 17
[0144] Compared with Example 14, the only difference is that the two-dimensional tellurene is doped with iodine vapor, and the solid iodine is heated to 38° C. to sublimate the solid iodine into iodine vapor for 5 hours.
[0145] The transfer characteristic curve corresponding to the two-terminal device prepared in Example 17 is obtained. By observing the transfer characteristic curve, it can be seen that the device prepared in Example 17 exhibits N-type semiconductor characteristics, indicating that Example 17 successfully converts P-type tellurene into an N-type semiconductor through iodine vapor doping.
[0146] Embodiment 18
[0147] Compared with Example 14, the only difference is that the two-dimensional tellurene is doped with iodine vapor, and the solid iodine is heated to 40° C. to sublimate the solid iodine into iodine vapor for 8 hours.
[0148] The transfer characteristic curve corresponding to the two-terminal device prepared in Example 18 is obtained. By observing the transfer characteristic curve, it can be seen that the device prepared in Example 18 exhibits N-type semiconductor characteristics, indicating that Example 18 successfully converts P-type tellurene into an N-type semiconductor through iodine vapor doping.
[0149] Embodiment 19
[0150] Compared with Example 14, the only difference is that the two-dimensional tellurene is doped with iodine vapor, and the solid iodine is heated to 42° C. to sublimate the solid iodine into iodine vapor for 5 hours.
[0151] The transfer characteristic curve corresponding to the two-terminal device prepared in Example 19 is obtained. By observing the transfer characteristic curve, it can be seen that the device prepared in Example 19 exhibits N-type semiconductor characteristics, indicating that Example 19 successfully converts P-type tellurene into an N-type semiconductor through iodine vapor doping.
[0152] Embodiment 20
[0153] Compared with Example 14, the only difference is that the two-dimensional tellurene is doped with iodine vapor, and the solid iodine is heated to 44° C. to sublimate the solid iodine into iodine vapor for 6 hours.
[0154] The transfer characteristic curve corresponding to the two-terminal device prepared in Example 20 is obtained. By observing the transfer characteristic curve, it can be seen that the device prepared in Example 20 exhibits N-type semiconductor characteristics, indicating that Example 20 successfully converts P-type tellurene into an N-type semiconductor through iodine vapor doping.
[0155] Embodiment 21
[0156] Compared with Example 14, the only difference is that the two-dimensional tellurene is doped with iodine vapor, and the solid iodine is heated to 45° C. to sublimate the solid iodine into iodine vapor for 4 hours.
[0157] The transfer characteristic curve corresponding to the two-terminal device prepared in Example 21 is obtained. By observing the transfer characteristic curve, it can be seen that the device prepared in Example 21 exhibits N-type semiconductor characteristics, indicating that Example 21 successfully converts P-type tellurene into an N-type semiconductor through iodine vapor doping.
[0158] It is worth mentioning that an embodiment of the present invention further provides a chip, which may include a chip body and the N-type tellurene field effect transistor in the above embodiment, wherein the N-type tellurene field effect transistor is arranged on the chip body.
[0159] An embodiment of the present invention further provides a circuit, which may include a circuit board body and the chip in the above embodiment, wherein the circuit is arranged on the circuit board body.
[0160] An embodiment of the present invention further provides a device, which may include a housing and the circuit in the above embodiment, wherein the circuit is arranged on the housing.
[0161] Those skilled in the art will readily appreciate other embodiments of the present application after considering the description and practicing the contents disclosed herein. The present application is intended to cover any variations, uses or adaptations of the present application, which follow the general principles of the present application and include common knowledge or customary technical means in the art that are not disclosed in the present application. The description and examples are intended to be exemplary only.
[0162] It should be understood that the present application is not limited to the exact construction that has been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof.
Claims
1. A method for preparing N-type tellurene based on iodine vapor doping method, characterized in that: The preparation method comprises: Providing two-dimensional tellurene; Two-dimensional tellurene is placed in a closed cavity and doped with iodine vapor to obtain N-type tellurene; wherein, doping the two-dimensional tellurene with iodine vapor includes: heating solid iodine to 30°C~45°C to sublimate the solid iodine into iodine vapor for 4-9 hours.
2. The method for preparing N-type tellurene based on iodine vapor doping method according to claim 1, characterized in that: Doping two-dimensional tellurene with iodine vapor includes heating solid iodine to 30° C. to sublimate solid iodine into iodine vapor for 5 hours.
3. An N-type tellurene, characterized in that: It is prepared by the preparation method of N-type tellurene based on iodine vapor doping method as described in claim 1 or 2.
4. A method for preparing an N-type tellurene field effect transistor based on iodine vapor doping method, characterized in that: The preparation method comprises: Providing two-dimensional tellurene; Placing two-dimensional tellurene on a silicon / silicon dioxide substrate with a back electrode to obtain a first sample; Prepare a source electrode and a drain electrode at both ends of the first sample; The first sample is placed upside down in a sealed cavity, and two-dimensional tellurene is doped with iodine vapor to obtain N-type tellurene, and the N-type tellurene is used as a gate; wherein the two-dimensional tellurene is doped with iodine vapor, including: heating solid iodine to 30° C. to 45° C. to sublimate the solid iodine into iodine vapor for 4 to 9 hours; An oxide film is formed on the surface of N-type tellurene to obtain a gate dielectric.
5. The method for preparing an N-type tellurene field effect transistor based on iodine vapor doping method according to claim 4, characterized in that: Gold / palladium electrodes were used for both the source and drain.
6. The method for preparing an N-type tellurene field effect transistor based on iodine vapor doping method according to claim 5, characterized in that: Doping two-dimensional tellurene with iodine vapor includes heating solid iodine to 30° C. to sublimate solid iodine into iodine vapor for 5 hours.
7. An N-type tellurene field effect transistor, characterized in that: The N-type tellurene comprises the N-type tellurene described in claim 3 or is prepared by the method for preparing an N-type tellurene field effect transistor based on iodine vapor doping method described in any one of claims 4 to 6.
8. A chip, characterized in that: It comprises a chip body and the N-type tellurene field effect transistor as claimed in claim 7, wherein the N-type tellurene field effect transistor is arranged on the chip body.
9. A circuit, characterized in that: The invention comprises a circuit board body and the chip as claimed in claim 8, wherein the chip is arranged on the circuit board body.
10. A device, characterized in that: The invention comprises a housing and the circuit according to claim 9, wherein the circuit is arranged on the housing.