Agglomerated diamond and its preparation method and application
Through the suspension dispersion granulation and sintering methods, the problems of poor spherical stylisation and sintering and lumping of agglomerated abrasives are solved, and efficient grinding and polishing and maximum strength are achieved.
Patent Information
- Application Number
- CN202310996210.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-08-08
AI Technical Summary
The spherical morphology of existing agglomerated abrasives is poor, which affects the grinding and polishing effect, and is prone to agglomeration during sintering, resulting in poor spherical morphology.
The gel is prepared by the sol-gel method by the sol-gel method, and spheroidized and sintered under the action of gas to ensure the spherical shape and dispersion of agglomerated diamonds, and the pore-forming agent ratio is adjusted to control the Self-sharp nature.
The excellent spherical shape of agglomerated diamond is achieved, the grinding and polishing effect is improved, the agglomeration problem is avoided during sintering, and the sintering strength is maximized by adjusting the pore-forming agent ratio.
Smart Images

Figure CN117003581B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of superhard material preparation, and in particular relates to agglomerated diamond and a preparation method and application thereof. Background Art
[0002] With the development of rail transit, 5G communication technology and the continuous emergence of new materials, the requirements for workpiece processing accuracy in various fields are getting higher and higher, and ultra-precision grinding and polishing technology has become a hot topic of current research. Grinding tools with high grinding efficiency, low environmental pollution and low surface roughness have become a new development trend. Ordinary diamonds have serious shortcomings in the field of precision machining due to the influence of self-sharpening and cutting depth. Spherical diamond agglomerated abrasives can maintain high grinding force without scratching during the grinding and polishing process by utilizing the characteristics of spherical multi-edge angles. They have begun to be used in the grinding of hard and brittle materials such as sapphire, silicon carbide, and gallium nitride. Stacked abrasives, also known as agglomerated abrasives, are small and irregular abrasives bonded together with ceramic binders or resin binders to form abrasives with a certain size, shape and strength. Compared with ordinary abrasives, after grinding, the abrasives on the surface of the agglomerated abrasives are passivated. Under a certain pressure, the passivated abrasives will fall off from the agglomerated abrasives, and the newly exposed abrasives will continue to participate in grinding, thereby reducing dressing. Currently, most stacked abrasives are prepared by rubbing screens or crushing methods, and their sphericity is poor, which is not conducive to grinding and polishing. Therefore, this type of spherical agglomerated diamond still needs further research and exploration. Summary of the invention
[0003] The object of the present invention is to provide agglomerated diamond and its preparation method and application. The preparation method of the present invention ensures the sphericity of agglomerated diamond through a special suspension dispersion granulation method and a suspension dispersion sintering method, avoiding the poor sphericity caused by ordinary crushing granulation, and the ordinary sintering (sintering in a container while stationary and aggregated) that causes the agglomerated diamond to be difficult to disperse during sintering, and the sintering temperature is too high, causing the agglomerated diamond to agglomerate and have poor sphericity. And the self-sharpening property of the agglomerated diamond can be further adjusted by adjusting the proportion of the pore-forming agent. The agglomerated diamond of the present invention has excellent sphericity, which is conducive to grinding and polishing. The present invention can solve the problem that the existing agglomerated abrasive (stacked abrasive) has poor sphericity and is not conducive to grinding and polishing.
[0004] To achieve the above object, the technical solution of the present invention is as follows:
[0005] In a first aspect, the present invention provides a method for preparing agglomerated diamonds, the preparation method comprising the following steps:
[0006] (1) mixing diamond and ceramic binder raw materials and obtaining a gel by a sol-gel method;
[0007] (2) drying, ball-milling, and sieving the gel to obtain a mixed powder;
[0008] (3) suspending the mixed powder by gas and keeping it dispersed, adding atomized slurry, wherein the slurry contains a binder and a modifier, and then contacting the atomized slurry with the mixed powder under the action of gas and spheroidizing them to obtain spherical diamond ceramic composite particles;
[0009] (4) Sintering the spherical diamond ceramic composite particles. During sintering, the spherical diamond ceramic composite particles are suspended and kept dispersed under the action of gas, and agglomerated diamonds are obtained after sintering.
[0010] Furthermore, in step (1), before mixing the diamond and the ceramic binder raw materials, a first dispersant is used to promote the dispersion of the diamond, the diamond is nano-scale diamond, and the mass ratio of the diamond to the first dispersant is 9 to 12:1.
[0011] Furthermore, in step (1), the mass percentages of the diamond and ceramic binder raw materials are 30-50%:50-70%.
[0012] Furthermore, in step (1), the ceramic binder raw material includes the following components in percentage by mass: 40-45% of tetraethyl orthosilicate, 15-20% of ethyl titanate, 2-4% of sodium nitrate, 4-16% of boric acid, 5-20% of aluminum nitrate, 1-3% of calcium nitrate and 3-5% of zinc nitrate.
[0013] Furthermore, in step (3) and / or step (4), the gas action is a flowing gas action.
[0014] Furthermore, in step (3), the slurry is added and atomized by pumping and air pressure injection, the pumping rate is 3-15 mL / min, the pressure of the air pressure injection is 0.3-2 MPa; and / or the flow rate of the gas action is 30-50 sccm; preferably, the gas source used in the air pressure injection includes one or more of air, nitrogen, argon, hydrogen, methane and ammonia. Mixed gas.
[0015] Furthermore, in step (3) and / or step (4), the gas source for exerting the gas effect includes one or a mixture of several gases selected from the group consisting of air, nitrogen, argon, hydrogen, methane and ammonia.
[0016] Further, in step (3), the adhesive comprises acrylate;
[0017] and / or, the modifier comprises one or more of a pore former, a second dispersant, a wetting agent and a modified powder, and the modified powder comprises a metal powder and / or a ceramic powder;
[0018] And / or, the slurry further comprises a solvent and optionally a small amount of the mixed powder in step (2).
[0019] Furthermore, the pore-forming agent includes one of polystyrene, polymethyl methacrylate, carbon black microspheres, polyvinyl alcohol or polyvinyl butyral;
[0020] and / or, the particle size of the pore-forming agent is 2 to 100 μm;
[0021] and / or, the mass of the pore former accounts for 5 to 15% of the total mass of the diamond and ceramic binder raw materials;
[0022] And / or, the metal powder includes one or more of cobalt, copper, aluminum, tin elemental powder or alloys thereof;
[0023] And / or, the ceramic powder includes one or more of silicon carbide, tungsten carbide and aluminum oxide;
[0024] And / or, in the slurry, by weight, the binder is 5-10%, the second dispersant is 0-2%, the wetting agent is 3-5%, the modified powder is 0-35%, the mixed powder is 0-5%, and the balance is solvent.
[0025] Furthermore, in step (4), the flow rate of the gas during sintering is 40-100 sccm;
[0026] And / or, the heating rate of the sintering is 4 to 8°C / min;
[0027] And / or, the sintering includes pre-sintering and high-temperature sintering, the pre-sintering temperature is kept at 100-120°C, 300-330°C, and 500-700°C for 60-180 minutes respectively, the high-temperature sintering temperature is kept at 650-920°C for 180-400 minutes, the spherical diamond ceramic composite particles are suspended and kept dispersed by gas during the high-temperature sintering, the spherical diamond ceramic composite particles are suspended and kept dispersed by gas during the pre-sintering, or, the spherical diamond ceramic composite particles are kept static and aggregated without gas action during the pre-sintering.
[0028] In a second aspect, the present invention provides an agglomerated diamond obtained by the above preparation method, wherein the agglomerated diamond comprises a ceramic binder and diamond, and the agglomerated diamond is spherical with a sphericity of 75-95%.
[0029] Furthermore, the particle size of the diamond is 50-250 nm; and / or the purity of the diamond is 95-98%.
[0030] Furthermore, the particle size of the agglomerated diamond is 50 to 2000 μm.
[0031] Furthermore, the ceramic binder is a titanium dioxide reinforced ceramic binder;
[0032] And / or, the porosity of the vitrified binder is no more than 30%.
[0033] In a third aspect, the present invention provides a use of the above-mentioned agglomerated diamond as an abrasive.
[0034] Furthermore, the application is the application of agglomerated abrasive, the application of abrasive for polishing liquid or the application of abrasive for polishing paste.
[0035] Furthermore, the grinding liquid comprises the following raw materials in percentage by mass: 10-15% of the above-mentioned agglomerated diamond, 5-10% of alkaline silicone oil, 10-15% of polyphosphoric acid, 10-15% of stabilizer, 3-5% of dithiothreitol, and 40-62% of distilled water.
[0036] The beneficial effects of the present invention are as follows:
[0037] (1) The preparation method of the present invention ensures the sphericity of the agglomerated diamond through a special suspension dispersion granulation method and suspension dispersion sintering method, thereby avoiding the poor sphericity caused by ordinary crushing granulation and the situation that the agglomerated diamond is difficult to disperse during sintering caused by ordinary sintering (sintering by stagnating and gathering in a container), the agglomerated diamond agglomerates and has poor sphericity due to the high sintering temperature. The spherical agglomerated diamond prepared by this method has excellent sphericity.
[0038] (2) The preparation method of the present invention also has the following advantages. First, the gel is prepared by the sol-gel method, which can not only disperse nano-scale diamonds well, but also dope and modify the ceramic binder well. Second, the suspension dispersion granulation can not only ensure the sphericity of the agglomerated diamonds, but also well control the particle size of the agglomerated diamonds, so that they can be large or small, and have a good coating structure from the inside to the outside, which is conducive to the passivation, consumption and use from the outside to the inside during grinding, and can also well modify its agglomeration structure during granulation, such as adding a pore-forming agent. The agglomerated structure can be re-poreed, and the self-sharpening property of the agglomerated diamond can be adjusted by adjusting the proportion of the pore-forming agent; thirdly, through suspended dispersion sintering, not only can the original shape (such as spherical multi-edge angles) and size (such as particle size) of the agglomerated diamond be guaranteed during high-temperature sintering, but also the heat transfer can be rapid and uniform, and is not limited to the sintering temperature. Debonding treatment can be carried out simultaneously during low-temperature sintering. The higher the temperature during high-temperature sintering, the greater the strength of the agglomerated diamond after sintering, so the maximum sintering strength of the spherical agglomerated diamond can be achieved.
[0039] (3) The agglomerated diamond of the present invention has excellent sphericity, which is beneficial for grinding and polishing.
[0040] (4) The agglomerated diamond of the present invention may be of nanometer grade, and the ceramic binder may be of a porous structure. The presence of the pores enables the agglomerated diamond to fully utilize the self-sharpening property and nanometer-grade diamond grinding in the grinding process, and can weaken the connection effect of the ceramic binder in the agglomerated diamond, so that the agglomerated diamond is gradually exposed, ground, passivated, and completely consumed from the outside to the inside as the grinding proceeds. In addition, the diamond particles and debris that are consumed by grinding can be accommodated to avoid damage such as grinding scratches. When the porosity does not exceed 30%, the structural strength of the agglomerated diamond can be guaranteed, and the self-sharpening property, utilization rate, and use effect of the agglomerated diamond can also be guaranteed.
[0041] (5) The agglomerated diamond of the present invention has a wide application range and good grinding effect when used. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is the SEM image of the agglomerated diamond obtained in Example 4 of the present invention. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. The embodiments of the present invention are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and processes are given, but the protection scope of the present invention is not limited to the following embodiments. Those skilled in the art should understand that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0044] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0045] In the present invention, unless otherwise specified and / or described, all numerical values involving the amount of components are "weight" from beginning to end. The process parameters in the following examples without specifying specific conditions are usually based on conventional conditions. The raw materials described in the following examples can all be obtained from public commercial channels.
[0046] According to a first aspect of the present invention, a method for preparing agglomerated diamonds comprises the following steps:
[0047] (1) mixing diamond and ceramic binder raw materials and obtaining a gel by a sol-gel method;
[0048] (2) drying, ball-milling, and sieving the gel to obtain a mixed powder;
[0049] (3) suspending the mixed powder by gas and keeping it dispersed, adding atomized slurry, wherein the slurry contains a binder and a modifier, and then contacting the atomized slurry with the mixed powder under the action of gas and spheroidizing them to obtain spherical diamond ceramic composite particles;
[0050] (4) Sintering the spherical diamond ceramic composite particles. During sintering, the spherical diamond ceramic composite particles are suspended and kept dispersed under the action of gas, and agglomerated diamonds are obtained after sintering.
[0051] In the preparation method of the present invention, the sphericity of the agglomerated diamond is ensured by a special suspension dispersion granulation method and a suspension dispersion sintering method, thereby avoiding the poor sphericity caused by ordinary crushing granulation, and the situation that the agglomerated diamond is difficult to disperse during sintering due to ordinary sintering (sintering in a container while stationary), the agglomerated diamond agglomerates and has poor sphericity due to the sintering temperature being too high. The preparation method of the present invention also has the following advantages. First, the gel is prepared by the sol-gel method, which can not only disperse nano-scale diamonds well, but also dope and modify the ceramic binder well. Second, the suspension dispersion granulation can not only ensure the sphericity of the agglomerated diamonds, but also well control the particle size of the agglomerated diamonds, so that they can be large or small, and have a good coating structure from the inside to the outside, which is conducive to the passivation, consumption and use from the outside to the inside during grinding, and can also well modify its agglomerated structure during granulation, such as adding a pore-forming agent to re-pore the agglomerated structure. Third, the suspension dispersion sintering can not only ensure the original shape (such as spherical multi-edge angle) and size (such as particle size) of the agglomerated diamonds during high-temperature sintering, but also can transfer heat quickly and evenly, and is not limited to the sintering temperature. Debonding treatment can be carried out simultaneously during low-temperature sintering. The higher the temperature during high-temperature sintering, the greater the strength of the agglomerated diamonds after sintering, so the maximum sintering of the strength of the spherical agglomerated diamonds can be achieved.
[0052] As an optional implementation, in step (1), the gel is obtained, and before mixing the diamond and ceramic binder raw materials, a first dispersant is used to promote diamond dispersion, the diamond is nano-scale diamond, and the mass ratio of the diamond to the first dispersant is 9 to 12:1 (for example, 9:1, 10:1, 11:1, 12:1).
[0053] As an optional embodiment, in step (1), obtaining the gel comprises the following steps:
[0054] S1, obtaining liquid A: diamond, anhydrous ethanol and a first dispersant are mixed evenly, and ethyl orthosilicate in the raw material of the ceramic binder is added, and the mixture is mixed evenly to obtain liquid A;
[0055] S2, obtaining liquid B: mixing ethyl titanate and anhydrous ethanol in the ceramic binder raw material evenly, adding distilled water and mixing evenly, obtaining liquid B;
[0056] S3, obtaining liquid C: uniformly mixing the remaining ceramic binder raw material and distilled water to obtain liquid C;
[0057] S4, obtaining a gel: adding liquid C to liquid A with stirring, then adding liquid B, mixing until a gel state is formed, and then standing for aging to obtain a gel.
[0058] The sol-gel method, mixing, drying, ball milling and the like in the preparation method of the present invention can all be realized by the prior art, wherein the mixing can be in one or more forms of stirring, oscillation and ultrasound, and when dispersing nano-scale diamonds, stirring methods such as magnetic mechanical stirring or ultrasonic mechanical stirring can be adopted. Since the diamonds are nano-scale, in order to make them disperse better, better ultrasonic mechanical stirring can be adopted, and the ultrasonic mechanical stirring dispersion time can be controlled to be 30 to 60 minutes (for example, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes, 60 minutes). In addition, in order to achieve a better gel state, in step S4, liquid C is stirred and added to liquid A to obtain a first mixed solution, and then the first mixed solution and liquid B are stirred for 3 to 5 hours (for example, 3 hours, 3.5 hours, 4 hours, 4.5 hours, and 5 hours), respectively, and then liquid B is added dropwise to the first mixed solution to obtain a second mixed solution. The second mixed solution is ultrasonically stirred at a temperature of 40 to 70°C (for example, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, and 70°C) until it reaches a gel state, and then the stirring is stopped, and the solution is allowed to stand and age for 24 hours to obtain a gel.
[0059] As an optional embodiment, in step (1), the mass percentage of diamond and ceramic binder raw materials is 30-50%:50-70% (for example, 30%:70%, 33%:67%, 35%:65%, 40%:60%, 43%:57%, 46%:54%, 50%:50%).
[0060] In the preparation method of the present invention, the proportion of diamond is controlled to be 30-50%, so that the prepared agglomerated diamond has high strength, long service life and good processing quality.
[0061] As an optional embodiment, in step (1), the ceramic binder raw material includes the following components in percentage by mass: 40-45% (e.g., 40%, 41%, 42%, 43%, 44%, 45%) of ethyl orthosilicate, 15-20% (e.g., 15%, 16%, 17%, 18%, 19%, 20%) of ethyl titanate, 2-4% (e.g., 2%, 2.5%, 3%, 3.5%, 4%) of ethyl orthosilicate, Sodium nitrate, 4-16% (e.g. 4%, 6%, 8%, 10%, 12%, 14%, 16%) boric acid, 5-20% (e.g. 5%, 7%, 9%, 11%, 13%, 15%, 17%, 19%, 20%) aluminum nitrate, 1-3% calcium nitrate (e.g. 1%, 1.5%, 2%, 2.5%, 3%) and 3-5% (e.g. 3%, 3.5%, 4%, 4.5%, 5%) zinc nitrate.
[0062] As an optional embodiment, in step (2), the drying temperature is 100-180°C (e.g., 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C).
[0063] As an optional embodiment, in step (2), the drying time is 10 to 15 hours (e.g., 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours);
[0064] As an optional embodiment, in step (2), the ball milling is carried out using zirconium oxide grinding balls with a particle size ratio of 40mm:20mm:10mm:5mm:2mm and a mass ratio of 0.5-1:0.5-1:0.5-1.5:0.5-1.5:0.5-1.5 (for example, 0.5:1:1.5:1.5:1.5, 0.7:0.9:1.1:1.1:1.1, 0.9:0.7:0.7:0.7:0.7, 1:0.5:0.5:0.5:0.5).
[0065] As an optional embodiment, in step (2), the ball milling time is 2 to 4 hours (e.g., 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours).
[0066] As an optional implementation, in step (2), the ball-to-material ratio of the ball mill is 0.5-1.5:0.5-1 (e.g., 0.5:1, 0.9:0.9, 1.3:0.7, 1.5:0.5).
[0067] As an optional embodiment, in step (2), the screening is performed using a 100# sieve.
[0068] As an optional implementation, in step (3) and / or step (4), the gas action is a flowing gas action.
[0069] In the preparation method of the present invention, the flow direction and speed of the gas are not limited, and it can be unidirectional flow, bidirectional flow, or multidirectional flow, and it can also be rotating flow, uniform flow, or variable speed flow.
[0070] As an optional embodiment, in step (3), the slurry is added and atomized by pumping and air pressure injection, the pumping rate is 3-15 mL / min (for example, 3 mL / min, 5 mL / min, 7 mL / min, 9 mL / min, 11 mL / min, 13 mL / min, 15 mL / min), and the pressure of the air pressure injection is 0.3-2 MPa (for example, 0.3 MPa, 0.5 MPa, 0.7 MPa, 0.9 MPa, 1.3 MPa, 1.5 MPa, 1.7 MPa, 1.9 MPa, 2 MPa).
[0071] The gas used in the preparation method of the present invention to play the role of gas and the gas pressure injection can be used as long as it does not react with the raw materials. Typical but not limited gases include one or more mixed gases of air, nitrogen, argon, hydrogen, methane and ammonia. Among them, the gas can be compressed or uncompressed, whichever allows the material to be suspended and dispersed. It should also be noted that flammable and explosive gases should not be used for sintering.
[0072] As an optional embodiment, in step (3), the flow rate of the gas is 30-50 sccm (for example, 30 sccm, 35 sccm, 40 sccm, 45 sccm, 50 sccm).
[0073] As an optional implementation, in step (3), the adhesive includes acrylic resin.
[0074] In the preparation method of the present invention, the acrylic resin typically but not limitedly includes BR73, BR113, BR115 or BR106. BR73 and similar numbers are brands of thermoplastic acrylic resins produced by Mitsubishi of Japan, which can be mixed with 30% toluene solution and used as a binder solution.
[0075] As an optional embodiment, in step (3), the modifier includes one or more of a pore former, a second dispersant, a wetting agent and a modified powder, and the modified powder includes metal powder and / or ceramic powder.
[0076] In the preparation method of the present invention, any dispersant, wetting agent and solvent that can respectively play the role of dispersing, wetting and dissolving can be used in the slurry. And the dispersant used in the present invention (including the first dispersant and / or the second dispersant) typically includes triethylhexyl phosphate, sodium dodecyl sulfate or sodium dodecylbenzene sulfonate, which can be mixed with 30% toluene solution and used as a dispersant solution; the wetting agent can be polyethylene glycol, typically including polyethylene glycol 1000 (PEG1000), polyethylene glycol 1500 (PEG1500) or polyethylene glycol 2000 (PEG2000) without limitation. The solvent typically includes isopropanol, ethyl acetate or n-butyl acetate, etc. without limitation.
[0077] As an optional embodiment, in step (3), the metal powder includes one or more of single metal powders such as cobalt, copper, tin, aluminum, or their alloy powders, and the ceramic powder includes one or more of silicon carbide, tungsten carbide, and aluminum oxide.
[0078] In the preparation method of the present invention, metal powder is used to particularly enhance the toughness of agglomerated diamond, and ceramic powder is used to particularly improve the brittleness of agglomerated diamond.
[0079] As an optional embodiment, in step (3), the slurry further includes a solvent and optionally a small amount of the mixed powder in step (2).
[0080] In the preparation method of the present invention, a small amount of mixed powder is added to the slurry so that the suspended and dispersed mixed powder can be better contacted with the slurry for spheroidization.
[0081] As an optional embodiment, in step (3), the pore-forming agent includes one or more of PS (polystyrene), PMMA (polymethyl methacrylate), carbon black microspheres, PVA (polyvinyl alcohol) or PVB (polyvinyl butyral); and / or the particle size of the pore-forming agent is 2 to 100 μm (for example, 2 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm); and / or the mass of the pore-forming agent accounts for 5 to 15% (for example, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%) of the total mass of the diamond and ceramic binder raw materials.
[0082] In the preparation method of the present invention, the self-sharpening property of the agglomerated diamond can be adjusted by adjusting the use and proportion of the pore-forming agent. When the pore-forming agent ratio is selected from the range, the agglomerated diamond has both good strength and self-sharpening property, and has a long service life. When it is below the range, the pore-forming agent has a small effect on the strength of the agglomerated diamond, and the self-sharpening property of the agglomerated diamond is poor during use. When the pore-forming agent ratio is higher than the range, the strength of the agglomerated diamond is low, the self-sharpening property is strong, but the service life is short. In addition, the pores in the ceramic binder generated by the pore-forming agent have a chip-accommodating capacity that increases with the increase in the size of the pore-forming agent.
[0083] As an optional embodiment, in step (3), in the slurry, by weight, the binder is 5-10% (for example, 5%, 6%, 7%, 8%, 9%, 10%), the second dispersant is 0-2% (for example, 0%, 0.5%, 1%, 1.5%, 2%), the wetting agent is 3-5% (for example, 3%, 3.5%, 4%, 4.5%, 5%), the modified powder is 0-35% (for example, 0%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%), the mixed powder is 0-5% (for example, 0%, 0.5%, 1%, 2%, 3%, 4%, 4.5%, 5%), and the balance is solvent.
[0084] As an optional embodiment, in step (4), the flow rate of the gas during sintering is 40-100 sccm (for example, 40 sccm, 50 sccm, 60 sccm, 70 sccm, 80 sccm, 90 sccm, 100 sccm).
[0085] In the preparation method of the present invention, during sintering, the gas effect can be exerted at the beginning of sintering to make the spherical diamond ceramic composite particles suspended and kept dispersed, or a low-temperature sintering can be performed first. In this case, during low-temperature sintering, the sintering temperature is relatively low, which will not cause the aggregated spherical diamond ceramic composite particles to agglomerate and change the sphericity. When the temperature reaches a level that can cause the spherical diamond ceramic composite particles to agglomerate, the gas effect is exerted in advance to make the spherical diamond ceramic composite particles suspended and kept dispersed, so as to avoid the agglomeration of the undispersed spherical diamond ceramic composite particles due to excessively high temperature and change the sphericity.
[0086] As an optional implementation, in step (4), the heating rate during sintering is 4 to 8°C / min (e.g., 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min).
[0087] As an optional embodiment, in step (4), the sintering includes pre-sintering and high-temperature sintering, and the pre-sintering temperature is 100-120°C (e.g., 100°C, 105°C, 110°C, 120°C), 300-330°C (e.g., 300°C, 305°C, 310°C, 315°C, 320°C, 325°C, 330°C), 500-700°C (e.g., 500°C, 505°C, 510°C, 515°C, 520°C, 525°C, 530°C), or 550-600°C (e.g., 550-600°C, 550-600°C). 5℃, 520℃, 525℃, 530℃, 535℃, 540℃, 545℃, 550℃, 600℃, 650℃, 700℃) and keep warm for 60-180min (for example, 60min, 80min, 90min, 100min, 110min, 120min, 130min, 150min, 180min) respectively; the high temperature sintering temperature is 650-920℃ (for example The spherical diamond ceramic composite particles are suspended and kept dispersed by gas during the high temperature sintering, and the spherical diamond ceramic composite particles are suspended and kept dispersed by gas during the pre-sintering, or, the spherical diamond ceramic composite particles are kept static and aggregated without gas action during the pre-sintering.
[0088] In the preparation method of the present invention, a specific sintering method is selected according to the selection of raw materials. When pre-sintering is required, gas action is selectively used or not used according to the maximum temperature of the pre-sintering. If the maximum temperature of the pre-sintering can cause the spherical diamond ceramic composite particles to agglomerate and destroy the spherical shape, gas action is used to suspend them and keep them in a dispersed state. If the maximum temperature of the pre-sintering does not cause the spherical diamond ceramic composite particles to agglomerate and destroy the spherical shape, then for the principle of energy saving, gas action is not used, but the spherical diamond ceramic composite particles are directly kept in a static and aggregated state for pre-sintering. It should be noted that the maximum temperature during pre-sintering is lower than the temperature during the subsequent high-temperature sintering.
[0089] According to a second aspect of the present invention, a kind of agglomerated diamond obtained by the above-mentioned preparation method comprises a ceramic binder and diamond, and the agglomerated diamond is spherical with a sphericity of 75-95% (for example, 75%, 77%, 79%, 81%, 83%, 85%, 87%, 90%, 93%, 95%).
[0090] The agglomerated diamond of the present invention is spherical in shape and has good sphericity, which is conducive to grinding and polishing.
[0091] As an optional embodiment, the diamond particle size is 50 to 250 nm (50 nm, 70 nm, 100 nm, 130 nm, 150 nm, 180 nm, 200 nm, 220 nm, 250 nm).
[0092] The diamonds used in the agglomerated diamonds of the present invention are nano-scale, which is beneficial to improving the surface quality of the processed workpiece, such as surface roughness, etc. The diamond particle size is selected between 50 and 250 nm, which ensures the surface quality of the processed workpiece and the processing efficiency.
[0093] As an optional embodiment, the purity of the diamond is 95-98% (e.g., 95%, 95.5%, 96%, 96.5%, 97%, 97.5%, 98%).
[0094] As an optional embodiment, the particle size of the agglomerated diamond is 50 to 2000 μm (e.g., 50 μm, 100 μm, 300 μm, 500 μm, 700 μm, 1000 μm, 1300 μm, 1500 μm, 1700 μm, 2000 μm).
[0095] As an optional implementation, the ceramic binder is a titanium dioxide reinforced ceramic binder.
[0096] In the agglomerated diamond of the present invention, the ceramic binder used is a titanium dioxide reinforced ceramic binder, and the titanium dioxide can enhance the strength of the ceramic binder itself and delay the passivation of the agglomerated diamond.
[0097] As an optional embodiment, the porosity of the ceramic binder does not exceed 30% (eg, 30%, 25%, 20%, 15%, 10%, 5%, 3%).
[0098] The agglomerated diamond of the present invention can be of nanometer level, and the ceramic binder can be of porous structure. The presence of pores can fully utilize the self-sharpening property and nanometer-level diamond grinding in the agglomerated diamond grinding process, and can weaken the connection effect of the ceramic binder in the agglomerated diamond, so that the agglomerated diamond is gradually exposed, ground, passivated, and completely consumed from the outside to the inside as the grinding proceeds. In addition, it can also accommodate diamond particles or debris that are reduced in grinding consumption, avoiding damage such as grinding scratches. The inventors found that when the porosity does not exceed 30%, it can not only ensure the structural strength of the agglomerated diamond, but also ensure the self-sharpening property, utilization rate and use effect of the agglomerated diamond.
[0099] In addition, the present invention does not limit the type of diamond, and diamond abrasives commonly used in the art may be used, typically but not limitedly including single crystal diamond powder, polycrystalline diamond powder or single crystal diamond powder with roughened particle surface.
[0100] According to a third aspect of the present invention, a use of the above-mentioned agglomerated diamond as an abrasive.
[0101] As an optional implementation, the application is the application of agglomerated abrasive.
[0102] As an optional implementation, the application is application as an abrasive in abrasive paste.
[0103] As an optional implementation, the application is application as an abrasive in a grinding liquid.
[0104] As an optional embodiment, the grinding liquid includes the following raw materials in mass percentage: 10-15% (e.g., 10%, 11%, 12%, 13%, 14%, 15%) of the above-mentioned agglomerated diamond, 5-10% (e.g., 5%, 6%, 7%, 8%, 9%, 10%) of alkaline silicone oil, 10-15% (e.g., 10%, 11%, 12%, 13%, 14%, 15%) of polyphosphoric acid, 10-15% (e.g., 10%, 11%, 12%, 13%, 14%, 15%) of stabilizer, 3-5% (e.g., 3%, 3.5%, 4%, 4.5%, 5%) of dithiothreitol, and 40-62% (e.g., 40%, 44%, 48%, 52%, 56%, 60%, 62%) of distilled water.
[0105] The agglomerated diamond of the present invention has a porous structure during grinding, so that it can give full play to its self-sharpening property, fully utilize nano-scale diamond grinding, and weaken the connecting effect of the ceramic binder in the agglomerated diamond, so that the agglomerated diamond is gradually exposed, ground, passivated, and completely consumed from the outside to the inside as the grinding proceeds. In addition, the agglomerated diamond can also accommodate diamond particles or debris that are reduced in grinding consumption, thereby avoiding damage such as grinding scratches.
[0106] The diamond used in the specific examples and comparative examples of the present invention was purchased from Yangling Meichang New Materials Co., Ltd. with a purity of 95-98%, and other raw materials were sourced from Jingchun Reagent.
[0107] The present invention will be further described in detail below with reference to specific embodiments.
[0108] Example 1
[0109] A method for preparing agglomerated diamond comprises the following steps:
[0110] (1) Mixing diamond and ceramic binder raw materials and obtaining a gel by a sol-gel method, the specific steps are as follows:
[0111] S1. Obtaining liquid A: subjecting 45 g of diamond with a particle size of 100 to 250 nm, anhydrous ethanol and 5 g of sodium dodecylbenzene sulfonate to ultrasonic mechanical stirring for 60 min to disperse the diamond; then adding 45 g of ethyl orthosilicate in the ceramic binder raw material to the above solution and stirring, which is marked as liquid A;
[0112] S2. Obtaining liquid B: Stir 19 g of ethyl titanate and anhydrous ethanol in the ceramic binder raw material, then add distilled water and continue stirring for standby use, marked as liquid B;
[0113] S3, obtaining liquid C: stirring the remaining 4 g of sodium nitrate, 15 g of boric acid, 10 g of aluminum nitrate, 2 g of calcium nitrate, 5 g of zinc nitrate and distilled water in the ceramic binder raw material, and marking it as liquid C;
[0114] S4. Obtaining a gel: adding liquid C into liquid A in a stirring state using a peristaltic pump to obtain a first mixed solution, stirring the first mixed solution and liquid B for 4 hours respectively, then using a peristaltic pump to drop liquid B into the first mixed solution to obtain a second mixed solution, placing the second mixed solution in a 55°C water bath for ultrasonic stirring, stopping stirring when the solution reaches a gel state, and allowing to stand for 24 hours to obtain a gel.
[0115] (2) The gel obtained in step (1) is placed in an oven at 120° C. and dried for 12 h, then crushed by ball milling, and sieved through a 100# sieve to obtain a mixed powder. During the ball milling, zirconium oxide grinding balls with a particle size ratio of 40 mm: 20 mm: 10 mm: 5 mm: 2 mm and a mass ratio of 0.5: 0.7: 1: 1.2: 1.5 are used for ball milling, the ball-to-material ratio is 1.5: 1, and the ball milling time is 3 h.
[0116] (3) dividing the mixed powder obtained in step (2) into two parts, wherein 95% of the mixed powder is blown up and kept dispersed by clean compressed air with a gas flow rate of 40 sccm, and at the same time, a slurry containing the remaining 5% of the mixed powder is transported to a spray gun at a rate of 10 mL / min by a peristaltic pump, and the spray gun uses 1.5 MPa of clean compressed air as a power to spray and atomize the slurry, and then the atomized slurry is brought into contact with the mixed powder and spheroidized under the flow of clean compressed air with a gas flow rate of 40 sccm to obtain spherical diamond ceramic composite particles;
[0117] The slurry is obtained by adding 10 g BR73, 2 g sodium dodecylbenzene sulfonate, 5 g PEG1500, 3 g aluminum powder, 5 g silicon carbide, 2 g alumina, 5% mixed powder and 21.75 g 50-80 μm carbon black microspheres to isopropanol solvent and mixing evenly to obtain 220 g slurry.
[0118] (4) drying the spherical diamond ceramic composite particles obtained in step (3), and then pre-sintering and degumming them at a heating rate of 6°C / min, and keeping them warm at 100°C, 300°C, and 550°C for 120 min respectively; then blowing the spherical diamond ceramic composite particles with clean compressed air at a gas flow rate of 80 sccm and keeping them dispersed, and then heating them to 700°C for high-temperature sintering, and keeping them warm for 240 min to obtain agglomerated diamonds.
[0119] Example 2
[0120] A method for preparing agglomerated diamond comprises the following steps:
[0121] (1) Mixing diamond and ceramic binder raw materials and obtaining a gel by a sol-gel method, the specific steps are as follows:
[0122] S1. Obtaining liquid A: subjecting 35 g of diamond with a particle size of 50 to 90 nm, anhydrous ethanol and 3 g of sodium dodecyl sulfate to ultrasonic mechanical stirring for 60 min to disperse the diamond; then adding 40 g of ethyl orthosilicate in the ceramic binder raw material to the above solution and stirring, which is marked as liquid A;
[0123] S2. Obtaining liquid B: Stir 15 g of ethyl titanate and anhydrous ethanol in the ceramic binder raw material, then add distilled water and continue stirring for standby use, marked as liquid B;
[0124] S3, obtaining liquid C: stirring the remaining 5g of sodium nitrate, 16g of boric acid, 15g of aluminum nitrate, 5g of calcium nitrate, 4g of zinc nitrate and distilled water in the ceramic binder raw material, and marking it as liquid C;
[0125] S4. Obtaining a gel: adding liquid C into liquid A in a stirring state using a peristaltic pump to obtain a first mixed solution, stirring the first mixed solution and liquid B for 4 hours respectively, then using a peristaltic pump to drop liquid B into the first mixed solution to obtain a second mixed solution, placing the second mixed solution in a 55°C water bath for ultrasonic stirring, stopping stirring when the solution reaches a gel state, and allowing to stand for 24 hours to obtain a gel.
[0126] (2) The gel obtained in step (1) is placed in an oven at 120° C. and dried for 12 h, then crushed by ball milling, and sieved through a 100# sieve to obtain a mixed powder. During the ball milling, zirconium oxide grinding balls with a particle size ratio of 40 mm: 20 mm: 10 mm: 5 mm: 2 mm and a mass ratio of 0.5: 0.7: 1: 1.2: 1.5 are used for ball milling, the ball-to-material ratio is 1.5: 1, and the ball milling time is 3 h.
[0127] (3) The mixed powder obtained in step (2) is all blown up and kept dispersed by clean compressed air with a gas flow rate of 30 sccm, and the slurry is transported to the spray gun at a rate of 5 mL / min by a peristaltic pump. The spray gun uses 0.5 MPa clean compressed air as a power to spray and atomize the slurry, and then the atomized slurry is brought into contact with the mixed powder and spheroidized under the flow of clean compressed air with a gas flow rate of 30 sccm to obtain spherical diamond ceramic composite particles;
[0128] The slurry is obtained by adding 10 g BR73, 2 g sodium dodecylbenzene sulfonate, 5 g PEG1500 and 13.5 g carbon black microspheres of 80-100 μm into an isopropanol solvent and mixing them evenly to obtain a slurry.
[0129] (4) drying the spherical diamond ceramic composite particles obtained in step (3), and then pre-sintering and degumming them at a heating rate of 6°C / min, and keeping them warm at 100°C, 300°C, and 500°C for 120 min respectively; then blowing the spherical diamond ceramic composite particles with clean compressed air at a gas flow rate of 45 sccm and keeping them dispersed, and then heating them to 600°C for high-temperature sintering, and keeping them warm for 240 min to obtain agglomerated diamonds.
[0130] Example 3
[0131] A method for preparing agglomerated diamond, which differs from Example 1 in that:
[0132] (3) The mixed powder obtained in step (2) is divided into two parts, wherein 95% of the mixed powder is blown up and kept dispersed by clean compressed air with an air flow rate of 50 sccm, and at the same time, a slurry containing the remaining 5% of the mixed powder is transported to a spray gun at a rate of 15 mL / min by a peristaltic pump, and the spray gun uses 1.8 MPa of clean compressed air as a power to spray and atomize the slurry, and then the atomized slurry is brought into contact with the mixed powder and spheroidized under the flow of clean compressed air with an air flow rate of 50 sccm to obtain spherical diamond ceramic composite particles;
[0133] The slurry is obtained by adding 10g BR73, 5g PEG1500, 3g cobalt powder, 5g tungsten carbide, 5% mixed powder and 12g 50-80μm polystyrene to isopropanol solvent and mixing them evenly to obtain slurry.
[0134] (5) drying the spherical diamond ceramic composite particles obtained in step (3), and then pre-sintering and degumming them at a heating rate of 6°C / min, and keeping them warm at 100°C, 300°C, and 550°C for 120 min respectively; then blowing the spherical diamond ceramic composite particles with clean compressed air at a gas flow rate of 100 sccm and keeping them dispersed, and then heating them to 750°C for high-temperature sintering, and keeping them warm for 240 min to obtain agglomerated diamonds.
[0135] The rest of the settings are the same as those in Example 1.
[0136] Example 4
[0137] A method for preparing agglomerated diamond, which differs from Example 1 in that no pore-forming agent is used, is as follows:
[0138] (3) Obtaining the slurry: According to the weight ratio, 10 g BR73, 2 g sodium dodecylbenzene sulfonate, 5 g PEG1500, 3 g aluminum powder, 5 g silicon carbide, 2 g aluminum oxide and 5% mixed powder were added to an isopropanol solvent and mixed evenly to obtain a slurry.
[0139] The rest of the settings are the same as those in Example 1.
[0140] Comparative Example 1
[0141] A method for preparing agglomerated diamonds, which differs from Example 1 in that a common mixing and granulation method is used, as follows:
[0142] (3) The mixed powder obtained in step (2) and the pore-forming agent carbon black microspheres are mixed in a three-dimensional mixer to obtain diamond ceramic composite particles.
[0143] The rest of the settings are the same as those in Example 1.
[0144] Comparative Example 2
[0145] A method for preparing agglomerated diamonds, which differs from Comparative Example 1 in that the diamonds are sintered in a static state and aggregated in a container, as follows:
[0146] (4) drying the diamond ceramic composite particles obtained in step (3), and then placing them in a crucible and sintering them in a muffle furnace at a heating rate of 6°C / min, and keeping them at 100°C, 300°C, and 550°C for 120 min respectively; then heating them to 700°C for high-temperature sintering, and keeping them at this temperature for 240 min to obtain agglomerated diamond.
[0147] The rest of the settings are the same as those in Comparative Example 1.
[0148] Tests and Results
[0149] (1) The agglomerated diamonds obtained in Examples 1-4 and Comparative Examples 1-2 were tested for sphericity and particle size using a laser particle size analyzer, and the porosity was measured using a nitrogen adsorption-desorption method (BET).
[0150] (2) The agglomerated diamonds obtained in Examples 1-4 and Comparative Examples 1-2 were used as abrasives in a grinding liquid to test their grinding ability.
[0151] The grinding liquid includes 15% agglomerated diamond, 10% alkaline silicone oil, 10% polyphosphoric acid, 12% stabilizer, 3% dithiothreitol and 50% distilled water.
[0152] During grinding, the grinding speed was controlled to be 50rpm, the grinding pressure to be 0.03MPa, the grinding time to be 2h, and the grinding object was single crystal silicon. After grinding, the surface roughness Ra of the single crystal silicon and the grinding efficiency and service life of the agglomerated diamond were tested and calculated. The service life refers to the use of agglomerated diamond to grind single crystal silicon. When the grinding efficiency and surface quality do not meet the requirements, it is considered that the service life of the agglomerated diamond has ended. At this time, the total number (pieces) of single crystal silicon ground during its entire use cycle is calculated.
[0153] The calculation method of surface roughness Ra is as follows: Use SJ-210 roughness meter to measure the surface roughness value Ra of single crystal silicon substrate, select 3 points at its center position and 2 cm circumference position from the center, measure 4 times in total, and then take the average value as the surface roughness value Ra of the single crystal silicon.
[0154] The calculation method of grinding efficiency is as follows: use a thickness gauge on a marble platform with a flatness level of 0 to measure the average thickness δ1 of 5 points on the initial single crystal silicon substrate and the average thickness δ2 of 5 points on the single crystal silicon substrate after grinding. The unit of the above workpiece thickness is μm, the grinding time is t, the unit is h, and the grinding efficiency of the material is ν = (δ1-δ2) / t, the unit is μm / h.
[0155] The specific grinding test results can be seen in Table 1.
[0156] Table 1
[0157] project life Surface roughness of workpiece Ra (μm) Grinding efficiency (μm / h) Example 1 500 pieces 0.003 15 Example 2 400 pieces 0.002 20 Example 3 300 pieces 0.002 10 Example 4 400 pieces 0.003 12 Comparative Example 1 160 tablets 0.005 5 Comparative Example 2 150 tablets 0.006 5
[0158] After testing, it was found that the agglomerated diamonds obtained in Examples 1-4 were spherical, with a sphericity of 75-95% and a particle size of 50-2000 μm. Figure 1 As shown, from Figure 1 It can be seen that the agglomerated diamond is spherical, most of the particles have a good spherical morphology, and the particle size is between 300 and 1100 μm. Through the test comparison of Example 1 and Example 4, it can be seen that the use of the pore-forming agent can increase the porosity of the ceramic binder in the agglomerated diamond, and the porosity increase does not exceed 30%, but the structural strength, self-sharpening, utilization rate and use effect of the agglomerated diamond obtained in Example 1 after pore formation are better than those in Example 4. This should be that the presence of pores in the ceramic binder can weaken the connection effect of the ceramic binder in the agglomerated diamond, so that the agglomerated diamond is gradually exposed, ground, passivated, and completely consumed from the outside to the inside as the grinding proceeds, and it can also accommodate diamond particles and debris that are reduced in grinding consumption, avoiding damage such as grinding scratches, so that the agglomerated diamond can give full play to its self-sharpening during the grinding process, and improve the utilization rate and use effect.
[0159] By comparing Example 1 with Comparative Example 1, it can be seen that since Comparative Example 1 adopts ordinary crushing granulation and mixed granulation, even if mixed granulation is performed after screening and the suspension dispersion sintering method of the present invention is adopted during sintering, due to the lack of good granulation shaping during mixing, although spherical agglomerated diamonds are obtained after sintering, the quantity is extremely small, and most of the agglomerated diamonds are non-spherical. It can be seen that the suspension dispersion granulation of the present invention is the key to ensuring the sphericity of the agglomerated diamonds. And by comparing Examples 1-4, it can be seen that the suspension dispersion granulation can also modify the agglomerated structure and performance during granulation, such as adding a pore-forming agent to re-pore the agglomerated structure, adding metal powder or ceramic powder to improve the performance of the agglomerated diamond, etc.
[0160] By comparing Example 1 with Comparative Example 2, it can be seen that since Comparative Example 2 does not use the suspension dispersion sintering method of the present invention during sintering, the agglomerated diamonds agglomerate after high-temperature sintering, and the spherical structure is destroyed. It can be seen that the suspension dispersion sintering of the present invention is the key to ensuring the sphericity of the agglomerated diamonds.
[0161] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are within the scope of protection of the pending claims of the present invention.
Claims
1. A method for preparing agglomerated diamond, characterized in that: The preparation method comprises the following steps: (1) mixing diamond and ceramic binder raw materials and obtaining a gel by a sol-gel method; (2) drying, ball-milling, and sieving the gel to obtain a mixed powder; (3) suspending the mixed powder and maintaining dispersion by gas action, adding atomized slurry, wherein the slurry contains a binder and a modifier, and then contacting the atomized slurry with the mixed powder under the action of gas and spheroidizing the mixed powder to obtain spherical diamond ceramic composite particles; (4) Sintering the spherical diamond ceramic composite particles. During sintering, the spherical diamond ceramic composite particles are suspended and kept dispersed under the action of gas, and agglomerated diamonds are obtained after sintering.
2. The preparation method according to claim 1, characterized in that In step (1), before mixing diamond and ceramic binder raw materials, a first dispersant is used to promote diamond dispersion, the diamond is nano-scale diamond, and the mass ratio of the diamond to the first dispersant is 9-12:
1.
3. The preparation method according to claim 1, characterized in that: In step (1), the mass percentage of the diamond and ceramic binder raw materials is 30-50%: 50-70%; And / or, in step (1), the ceramic binder raw material comprises the following components in percentage by mass: 40-45% of tetraethyl orthosilicate, 15-20% of ethyl titanate, 2-4% of sodium nitrate, 4-16% of boric acid, 5-20% of aluminum nitrate, 1-3% of calcium nitrate and 3-5% of zinc nitrate; And / or, in step (3) and / or step (4), the gas action is a flowing gas action.
4. The preparation method according to claim 1, characterized in that: In step (3), the slurry is added and atomized by pumping and air pressure injection, the pumping rate is 3-15 mL / min, the air pressure injection pressure is 0.3-2 MPa; and / or the gas flow rate is 30-50 sccm; And / or, in step (3) and / or step (4), the gas source for the gas to function includes one or a mixture of several gases selected from the group consisting of air, nitrogen, argon, hydrogen, methane and ammonia.
5. The preparation method according to claim 4, characterized in that: In step (3), the gas source used in the gas pressure spraying includes one or a mixture of several gases selected from the group consisting of air, nitrogen, argon, hydrogen, methane and ammonia.
6. The preparation method according to claim 1, characterized in that: In step (3), the adhesive comprises acrylate; and / or, the modifier comprises one or more of a pore former, a second dispersant, a wetting agent and a modified powder, and the modified powder comprises a metal powder and / or a ceramic powder; And / or, the slurry further includes a solvent and optionally a small amount of the mixed powder in step (2).
7. The preparation method according to claim 6, characterized in that: The pore-forming agent includes one or more of polystyrene, polymethyl methacrylate, carbon black microspheres, polyvinyl alcohol or polyvinyl butyral; And / or, the particle size of the pore-forming agent is 2 to 100 μm; and / or, the mass of the pore former accounts for 5-15% of the total mass of the diamond and ceramic binder raw materials; And / or, the metal powder includes one or more of cobalt, copper, aluminum, tin elemental powder or alloys thereof; And / or, the ceramic powder includes one or more of silicon carbide, tungsten carbide and aluminum oxide; And / or, in the slurry, by weight, the binder is 5-10%, the second dispersant is 0-2%, the wetting agent is 3-5%, the modified powder is 0-35%, the mixed powder is 0-5%, and the balance is solvent.
8. The preparation method according to claim 1, characterized in that: In step (4), the flow rate of the gas during sintering is 40-100 sccm; And / or, the heating rate of the sintering is 4-8°C / min; And / or, the sintering includes pre-sintering and high-temperature sintering, the pre-sintering temperature is kept at 100-120°C, 300-330°C, and 500-700°C for 60-180 minutes respectively, the high-temperature sintering temperature is kept at 650-920°C for 180-400 minutes, the spherical diamond ceramic composite particles are suspended and kept dispersed by gas during the high-temperature sintering, the spherical diamond ceramic composite particles are suspended and kept dispersed by gas during the pre-sintering, or, the spherical diamond ceramic composite particles are kept static and aggregated without gas action during the pre-sintering.
9. An agglomerated diamond obtained by the preparation method according to any one of claims 1 to 8, characterized in that: The agglomerated diamond comprises a ceramic binder and diamond, and the agglomerated diamond is spherical with a sphericity of 75-95%.
10. The agglomerated diamond according to claim 9, characterized in that: The particle size of the diamond is 50-250 nm; and / or the purity of the diamond is 95-98%; And / or, the particle size of the agglomerated diamond is 50-2000 μm; And / or, the ceramic binder is a titanium dioxide reinforced ceramic binder; And / or, the porosity of the ceramic binder is no more than 30%.
11. Use of the agglomerated diamond obtained by the preparation method according to any one of claims 1 to 8 or the agglomerated diamond according to any one of claims 9 to 10 as an abrasive.
Citation Information
Patent Citations
Perovskite / diamond composite material and preparation method
CN106299393A
Electromagnetic field atomization diamond abrasive particle uniform jetting device and method
CN106391347A
Preparation method of spherical diamond micro-powder abrasive
CN110484205A
Ultra-precision grinding wheel and manufacturing method thereof
CN115070626A
Production method for coating metal powder on surface of diamond
CN116393697A