A servo hot forming partition quenching method for an integrated complex component and a component

Through the servo hot forming process and zoned quenching technology, the design of heat transfer coefficient and mold gap is used to solve the zoned quenching problem of complex components in servo hot forming, achieving the adjustment of local mechanical properties and improving the forming quality, which satisfies the requirements of complex components. strength and crash performance requirements.

CN117210646BActive Publication Date: 2024-10-01WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311111145.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-29
Publication Date
2024-10-01
Estimated Expiration
2043-08-29

AI Technical Summary

Technical Problem

The existing technology is difficult to achieve zoned quenching during the servo hot forming process of integrated complex components, making it difficult to adjust local mechanical properties. Moreover, the traditional hot stamping process has problems such as uneven mold temperature distribution and affected formability.

Method used

By obtaining the design information of the target component, calculating the heat transfer coefficient and mold gap according to the manufacturing material, preparing the thermal insulation coating and mold, using the servo hot forming process for zone quenching, controlling the cooling rate and heat transfer conditions of each area, and achieving zone control Warm quenching.

Benefits of technology

It realizes the adjustment of local mechanical properties of one-piece complex components, improves the forming quality and strength, improves the collision performance, and avoids the problem of uneven mold temperature distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117210646B_ABST
    Figure CN117210646B_ABST
Patent Text Reader

Abstract

The present invention relates to a servo hot forming partition quenching method for an integrated complex component and a component. First, the design information of the target component is obtained, and then the heat transfer coefficient and mold gap corresponding to each partition are obtained according to the manufacturing material. Then, the blank is made according to the design information and a thermal insulation coating is coated on the surface of each partition respectively. Finally, a mold is made according to the mold gap, and servo hot forming partition quenching is performed to obtain the formed target component. Compared with the prior art, the present invention changes the heat transfer coefficient between each area of ​​the blank and the mold by coating a thermal insulation coating with a thickness corresponding to the heat transfer coefficient, and cooperates with different mold intervals between the mold and the blank. At the same time, the formability of the integrated complex component is improved through the servo hot forming process, and the cooling rate of the blank in each area during the forming process is controlled, thereby realizing partition temperature controlled quenching, and achieving the purpose of adjusting the local mechanical properties, so that the manufactured integrated complex component has both sufficient strength and good collision performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of high-performance component forming and manufacturing, and in particular to a servo hot forming partition quenching method for an integrated complex component and a component. Background Art

[0002] Lightweighting of automobiles can effectively save energy, reduce emissions and reduce consumption, and is an important way to achieve the country's dual carbon goals and the sustainable development of the automobile industry. In order to improve the level of automobile lightweighting technology, body components are developing in the direction of larger size, more complex structure, more controllable performance and more integrated manufacturing.

[0003] With the increase in component size and structural complexity, hot stamping parts with a single strength can no longer meet the requirements of forming manufacturing and collision energy absorption. Take the door ring as an example. As a typical large-size, complex structured integrated body component, the traditional door ring is composed of A-pillars, roof side beams, B-pillars and door sills, which are spot welded end to end to form a closed loop. The components are formed by hot stamping process. The A-pillars, roof side beams, B-pillars and door sills are all full martensite structures. Although the strength of the door ring is significantly improved, the buffering performance of the car is poor when the car is hit from the side, which can easily cause the car to roll over. In addition, the deformation and damage of the door ring are uncontrolled, which may cause secondary collisions due to large deformation or rupture of the upper part of the door ring, threatening the life safety of the driver and passengers. In order to solve the above problems, a laser welding door ring that can meet the collision requirements has been developed. The door ring selects different materials for welding to meet the collision strength requirements of different regions, but the material selection is complex, the overall hot stamping forming control is difficult, and the weld performance between dissimilar materials is low, which usually becomes a weak area for the door ring to fail in collision, resulting in insufficient overall strength. When using an integrated door ring made of the same material to ensure overall strength, although there is a hot stamping forming process that adjusts the mold temperature to change the cooling rate of different areas of the door ring to achieve customized mechanical properties of the door ring, the existing method has a complex mold water channel structure and has high requirements for temperature control accuracy and interface insulation in different areas, which may affect the forming performance of the door ring due to uneven mold temperature distribution.

[0004] In addition, since one-piece components are generally large in size and complex in structure, the local temperature of the plate often drops too quickly after the overall heating before forming, and the uneven temperature distribution of the component leads to cracking or excessive thinning. Servo hot forming can form the plate at a high temperature through an appropriate and high pressure head rate, achieving high-efficiency and high-precision forming and manufacturing of components, but it is currently only used for components with simple structures and single mechanical properties, and there is a lack of servo hot forming partition quenching methods for one-piece complex components. Therefore, there is an urgent need for a method that can perform partition quenching on one-piece complex components during servo hot forming to adjust local mechanical properties. Summary of the invention

[0005] In view of this, it is necessary to provide a method for partitioned quenching of servo hot forming of an integrated complex component and a component to solve the problem in the prior art of how to perform partitioned quenching on an integrated complex component to adjust local mechanical properties when performing servo hot forming on the component.

[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a method for servo hot forming and zone quenching of an integrated complex component, comprising:

[0008] Acquire design information of a target component, the target component comprising a plurality of partitions, the design information comprising a manufacturing material of the target component;

[0009] According to the manufacturing material, a heat transfer coefficient and a mold gap corresponding to each partition are obtained;

[0010] According to the heat transfer coefficient, the thickness of the thermal insulation coating corresponding to each partition is obtained;

[0011] Manufacturing a blank according to the design information, and coating a thermal insulation coating on the surface of each partition based on the thickness of the thermal insulation coating corresponding to each partition;

[0012] A mold is made according to the mold gap corresponding to each partition, the blank is servo hot formed by the mold, and the partition quenching is performed based on the thermal insulation coating with a thickness corresponding to the heat transfer coefficient on the surface of each partition to obtain the formed target component.

[0013] Furthermore, the design information also includes a target strength of each partition; and obtaining the heat transfer coefficient and mold gap corresponding to each partition according to the manufacturing material includes:

[0014] According to the manufacturing material, a heat transfer coefficient-strength performance relationship diagram and a mold gap-strength performance relationship diagram of the manufacturing material are obtained;

[0015] According to the target strength of each partition, based on the heat transfer coefficient-strength performance relationship diagram, the heat transfer coefficient corresponding to each partition is obtained;

[0016] According to the target strength of each partition, based on the mold gap-strength performance relationship diagram, the mold gap corresponding to each partition is obtained.

[0017] Furthermore, a patch plate is welded to the partition where the position in the target component that needs to be strengthened is located. The patch plate is annular, and the welding points between the patch plate and the target component are arranged with variable spacing.

[0018] Furthermore, the multiple partitions include a hard zone, a transition zone and a soft zone, the target strength of the hard zone is greater than the target strength of the transition zone, and the target strength of the transition zone is greater than the target strength of the soft zone; the hard zone is welded to connect the patch plate; the thickness of the thermal insulation coating is inversely proportional to the target strength.

[0019] Further, the blank is manufactured according to the design information, and the thermal insulation coating is applied to the surface of each partition based on the thickness of the thermal insulation coating corresponding to each partition, including:

[0020] Making the blank according to the design information, and spot welding the patch plate on the blank;

[0021] Based on the thickness of the thermal insulation coating corresponding to each partition, respectively apply the thermal insulation coating on the surface of each partition of the blank;

[0022] Allowing the blank coated with the heat-insulating coating to dry naturally for the first time, and then baking it for the first time;

[0023] Stop the first baking, and after the blank is cooled to room temperature, spray a high-temperature sealing reinforcing agent on the outside of the thermal insulation coating;

[0024] The blank coated with the high temperature seal reinforcing agent is naturally dried for a second time and then baked for a second time.

[0025] Furthermore, the mold is manufactured according to the mold gap corresponding to each partition, the blank is servo hot-formed by the mold, and the thermal insulation coating with a thickness corresponding to the heat transfer coefficient on the surface of each partition is quenched in the partition to obtain the formed target component, including:

[0026] The mold is manufactured according to the mold gap corresponding to each partition;

[0027] Setting initial hot forming process parameters, and optimizing the initial hot forming process parameters based on a genetic algorithm to obtain target hot forming process parameters;

[0028] According to the target hot forming process parameters, a servo process curve is obtained;

[0029] According to the servo process curve, the blank is subjected to servo hot forming through the die, and partition quenching is performed on the thermal insulation coating with a thickness corresponding to the heat transfer coefficient on each partition surface to obtain the formed target component.

[0030] Furthermore, the servo process curve includes:

[0031] S(t)=αt 3 +βt 2 +γt+η

[0032] Among them, S(t) is the displacement of the pressure head in the servo press, t is time, and α, β, γ and η are different adjustment coefficients.

[0033] Further, the servo hot forming is performed on the blank through the die according to the servo process curve, and the thermal insulation coating with a thickness corresponding to the heat transfer coefficient on each partition surface is subjected to partition quenching to obtain the formed target component, including:

[0034] The billet is heated and kept warm in a heating furnace to be completely austenitized;

[0035] Transfer and position the austenitized billet onto the die;

[0036] According to the servo process curve, the mold is closed based on a servo press to form the austenitized blank;

[0037] Based on the servo press, the pressure on the die is maintained, and the formed blank is subjected to zoned temperature-controlled quenching;

[0038] The pressure of the servo press is unloaded, the blank after zone temperature-controlled quenching is taken out, and trimming and punching are performed to obtain the target component.

[0039] Further, in the target component, the blank thickness of the hard zone is 1.0mm-2.0mm, and the target strength of the hard zone is tensile strength, ranging from 1300MPa-2000MPa; the blank thickness of the transition zone is 1.0mm-2.0mm, and the target strength of the transition zone is tensile strength, ranging from 1000MPa-1300MPa; the blank thickness of the soft zone is 1.0mm-2.0mm, and the target strength of the soft zone is tensile strength, ranging from 600MPa-1200MPa; the blanks are connected by laser welding, the welding current of the laser welding is 50A-300A, the laser pulse frequency is 20Hz-50Hz, the laser pulse width is 2.5ms-5.0ms, and the welding speed is 100mm / min-370mm / min;

[0040] The thickness of the patch plate is 1.0 mm-2.0 mm, the tensile strength of the patch plate is 1300 MPa-2000 MPa, and the patch plate is connected to the blank by spot welding;

[0041] The material of the thermal insulation coating is high-temperature reflective thermal insulation nano-composite ceramic coating GN-302A. When applying the thermal insulation coating, the first natural drying time is 20min-40min, the first baking temperature is 400℃-700℃, and the first baking time is 20min-40min; the high-temperature sealing reinforcing agent is F2A, the second natural drying time is 10min-30min, the second baking temperature is 250℃-300℃, and the second baking time is 10min-30min;

[0042] The heating temperature of the heating furnace is 900℃-950℃, and the holding time is 3min-5min; the time for transferring and positioning the billet on the mold is 3s-8s; the temperature of the mold is 20℃-150℃, and the mold gap is 0mm-0.2mm; the pressure on the mold is maintained at 1000KN-3500KN, and the zone temperature control quenching time is 5s-20s.

[0043] In a second aspect, the present invention further provides an integrated complex component manufactured by any of the integrated complex component servo hot forming zone quenching methods described above.

[0044] The present invention provides a servo hot forming and partition quenching method for an integrated complex component and a component. First, the design information of a target component is obtained, the target component includes a plurality of partitions, the design information includes the manufacturing material of the target component, and then the heat transfer coefficient and mold gap corresponding to each partition are obtained according to the manufacturing material. Then, the thickness of the thermal insulation coating corresponding to each partition is obtained according to the heat transfer coefficient. Then, a blank is manufactured according to the design information, and a thermal insulation coating is coated on the surface of each partition based on the thickness of the thermal insulation coating corresponding to each partition. Finally, a mold is manufactured according to the mold gap corresponding to each partition, the blank is servo hot formed by the mold, and partition quenching is performed based on the thermal insulation coating thickness corresponding to the surface of each partition and the heat transfer coefficient, so as to obtain the formed target component. Compared with the prior art, the present invention changes the heat transfer coefficient between each area of ​​the blank and the mold by applying a thermal insulation coating with a thickness corresponding to the heat transfer coefficient, and at the same time cooperates with different mold spacings between the mold and the blank. At the same time, the formability of the one-piece complex component is improved through a servo hot forming process, and the cooling rate of the blank in each area during the forming process is controlled, thereby realizing zoned temperature controlled quenching and achieving the purpose of adjusting local mechanical properties, so that the manufactured one-piece complex component has both sufficient strength and good collision performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 A method flow chart of an embodiment of a servo hot forming partition quenching method for an integrated complex component provided by the present invention;

[0046] Figure 2 for Figure 1 A method flow chart of an embodiment of step S102;

[0047] Figure 3 A schematic diagram of the front structure of a door ring blank with a patch plate in an embodiment of a servo hot forming and zone quenching method for an integrated complex component provided by the present invention;

[0048] Figure 4 A schematic diagram of the reverse structure of a door ring blank with a patch plate in an embodiment of a servo hot forming partition quenching method for an integrated complex component provided by the present invention;

[0049] Figure 5 A schematic diagram of the arrangement of welding points of a patch plate in an embodiment of a servo hot forming partition quenching method for an integrated complex component provided by the present invention;

[0050] Figure 6 A heat transfer coefficient-strength performance relationship diagram in an embodiment of a servo hot forming partition quenching method for an integrated complex component provided by the present invention;

[0051] Figure 7 A diagram showing the relationship between die gap and strength performance in an embodiment of a servo hot forming partition quenching method for an integrated complex component provided by the present invention;

[0052] Figure 8 A servo process curve in an embodiment of a servo hot forming partition quenching method for an integrated complex component provided by the present invention;

[0053] Fig. 9 This is a cloud diagram of the tensile strength distribution of the door ring during hot stamping in one embodiment of the servo hot forming and zone quenching method for an integrated complex component provided by the present invention. DETAILED DESCRIPTION

[0054] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0055] Before describing the specific embodiments, some technical terms in this article are first explained:

[0056] Servo thermoforming is an advanced thermoforming technology that combines servo control and thermoforming processes. It uses a servo control system to accurately control the forming temperature and forming force to achieve high-precision and high-efficiency thermoforming processing. In traditional thermoforming processes, there are usually difficulties in controlling temperature and force. However, servo thermoforming technology can achieve high-efficiency and high-precision forming of high-temperature plates in a shorter time by accurately controlling the forming force and forming temperature, avoiding cracking or excessive thinning caused by local cooling of the plate. Servo thermoforming technology is widely used in metal forming, plastic forming and composite material forming. Servo thermoforming is usually achieved by applying pressure to the mold using a servo press while controlling the temperature.

[0057] Partition quenching is a metal heat treatment process that aims to achieve an optimized combination of organization and performance by controlling the quenching and partitioning steps. During the partition quenching process, the material is first heated to a high temperature (complete austenitization) and then rapidly cooled (quenched) to form a high-hardness martensitic structure. Next, the material is tempered (drying heat treatment) before the martensite transforms to bainite to reduce hardness, reduce brittleness and increase toughness. Subsequently, the partition treatment is carried out for a short time before the bainite is formed, that is, it is kept at a higher temperature for a period of time. This helps to enrich the distribution of carbon in bainite at the right time and temperature by regressing the carbon concentration distribution, thereby increasing the strength and durability of the material. Through the partition quenching process, materials with excellent strength, toughness and impact toughness can be obtained, as well as high deformation capacity and fatigue life. This process is often used in the fields of automobile manufacturing, aerospace, tool manufacturing, etc. that require high-strength and high-toughness materials.

[0058] It is understandable that other technical terms, English abbreviations, etc. appearing in the following text are all prior art, and those skilled in the art can understand their meanings according to the context, and will not be explained in detail in this article due to space constraints.

[0059] In the description of the present application, “plurality” means two or more than two, unless otherwise clearly and specifically defined.

[0060] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0061] The present invention provides a servo hot forming zone quenching method for an integrated complex component and a component, which are described below respectively.

[0062] Combination Figure 1 As shown, a specific embodiment of the present invention discloses a servo hot forming partition quenching method for an integrated complex component, which specifically includes:

[0063] S101, obtaining design information of a target component, wherein the target component includes a plurality of partitions, and the design information includes a manufacturing material of the target component;

[0064] S102, obtaining a heat transfer coefficient and a mold gap corresponding to each partition according to the manufacturing material;

[0065] S103, obtaining the thickness of the thermal insulation coating corresponding to each partition according to the heat transfer coefficient;

[0066] S104, manufacturing a blank according to the design information, and coating a thermal insulation coating on the surface of each partition based on the thickness of the thermal insulation coating corresponding to each partition;

[0067] S105, manufacturing a mold according to the mold gap corresponding to each partition, performing servo hot forming on the blank through the mold, and performing partition quenching based on the thermal insulation coating with a thickness corresponding to the heat transfer coefficient on the surface of each partition to obtain the formed target component.

[0068] Compared with the prior art, the present invention changes the heat transfer coefficient between each area of ​​the blank and the mold by applying a thermal insulation coating with a thickness corresponding to the heat transfer coefficient, and at the same time cooperates with different mold spacings between the mold and the blank. At the same time, the formability of the one-piece complex component is improved through a servo hot forming process, and the cooling rate of the blank in each area during the forming process is controlled, thereby realizing zoned temperature controlled quenching and achieving the purpose of adjusting local mechanical properties, so that the manufactured one-piece complex component has both sufficient strength and good collision performance.

[0069] It should be noted that the target component in the present invention is an integrated complex component that is expected to be manufactured when the method is implemented, specifically an integrated door ring in an automobile part.

[0070] In a preferred embodiment, in the above step S101, the manufacturing material is selected as ultra-high-strength steel, the target component is partitioned and the number and position of welds are designed; at the same time, strength-thickness matching design is carried out to determine the hard zone, transition zone and soft zone, and select a strength-thickness combination with excellent collision performance to finally obtain the above design information.

[0071] Furthermore, in a preferred embodiment, a patch plate is welded to the partition of the target component where the position to be strengthened is located, the patch plate is annular, and the welding points between the patch plate and the target component are arranged with variable spacing. The patch plate can locally strengthen the integrated target component, and its annular design and the arrangement of welding points with variable spacing can further improve its anti-collision performance.

[0072] In a preferred embodiment, the target strength of the hard zone is greater than the target strength of the transition zone, and the target strength of the transition zone is greater than the target strength of the soft zone. The hard zone is welded to connect the patch plate to prevent it from breaking or secondary deformation when impacted, thereby ensuring its good anti-collision performance.

[0073] Combination Figure 2 As shown, in a preferred embodiment, the design information also includes the target strength of each partition; the above step S102, according to the manufacturing material, obtains the heat transfer coefficient and mold gap corresponding to each partition, specifically including:

[0074] S201, obtaining a heat transfer coefficient-strength performance relationship diagram and a mold gap-strength performance relationship diagram of the manufacturing material according to the manufacturing material;

[0075] S202, according to the target strength of each partition, based on the heat transfer coefficient-strength performance relationship diagram, obtaining the heat transfer coefficient corresponding to each partition;

[0076] S203, according to the target strength of each partition and based on the mold gap-strength performance relationship diagram, obtain the mold gap corresponding to each partition.

[0077] The above heat transfer coefficient-strength performance relationship diagram and die gap-strength performance relationship diagram can be obtained based on a flat plate die hot stamping test on a flat plate made of manufacturing material. The specific process is prior art and will not be described in detail in this article.

[0078] Furthermore, in a preferred embodiment, in the above step S103, the thickness of the thermal insulation coating corresponding to each partition is obtained according to the heat transfer coefficient, and the thickness of the thermal insulation coating is inversely proportional to the target strength. The thickness of the thermal insulation coating is used to control the cooling rate of a partition in the target component, and the partition temperature-controlled quenching is achieved, thereby controlling the target strength that can be finally achieved.

[0079] Specifically, in a preferred embodiment, the above step S104, manufacturing a blank according to the design information, and coating the thermal insulation coating on the surface of each partition based on the thickness of the thermal insulation coating corresponding to each partition, specifically includes:

[0080] Manufacturing the blank according to the design information, and welding the patch plate to the blank;

[0081] Based on the thickness of the thermal insulation coating corresponding to each partition, respectively apply the thermal insulation coating on the surface of each partition of the blank;

[0082] Allowing the blank coated with the heat-insulating coating to dry naturally for the first time, and then baking it for the first time;

[0083] Stop the first baking, and after the blank is cooled to room temperature, spray a high-temperature sealing reinforcing agent on the outside of the thermal insulation coating;

[0084] The blank coated with the high temperature seal reinforcing agent is naturally dried for a second time and then baked for a second time.

[0085] The above process can ensure that the thermal insulation coating has a good thermal insulation effect and will not fail during processes such as mold closing.

[0086] Further, in a preferred embodiment, the above step S105, manufacturing a mold according to the mold gap corresponding to each partition, performing servo hot forming on the blank through the mold, and performing partition quenching based on the thickness of the thermal insulation coating corresponding to the heat transfer coefficient on the surface of each partition to obtain the formed target component, specifically includes:

[0087] The mold is manufactured according to the mold gap corresponding to each partition;

[0088] Setting initial hot forming process parameters, and optimizing the initial hot forming process parameters based on a genetic algorithm to obtain target hot forming process parameters;

[0089] According to the target hot forming process parameters, a servo process curve is obtained;

[0090] According to the servo process curve, the blank is subjected to servo hot forming through the die, and partition quenching is performed on the thermal insulation coating with a thickness corresponding to the heat transfer coefficient on each partition surface to obtain the formed target component.

[0091] Specifically, in a preferred embodiment, the target hot forming process parameters include: forming temperature T is 650°C-900°C, the friction coefficient μ between the mold and the sheet is 0.1-0.5, and the forming speed v is 50mm / s-300mm / s.

[0092] Specifically, in a preferred embodiment, the servo process curve in the above process includes:

[0093] S(t)=αt 3 +βt 2 +γt+η

[0094] Among them, S(t) is the displacement of the pressure head in the servo press, t is time, and α, β, γ and η are different adjustment coefficients.

[0095] Servo hot forming is performed through this curve, and the flexible control characteristics of the servo press can be utilized. The multi-point free programming mode is adopted and the curve is drawn in the idle descending section and the servo forming section, taking into account the forming performance and forming efficiency of complex components.

[0096] Furthermore, in the above process, according to the servo process curve, the blank is servo hot formed by the die, and the thermal insulation coating with a thickness corresponding to the heat transfer coefficient on each partition surface is partitioned and quenched to obtain the formed target component, which specifically includes:

[0097] The billet is heated and kept warm in a heating furnace to be completely austenitized;

[0098] Transfer and position the austenitized billet onto the die;

[0099] According to the servo process curve, the mold is closed based on a servo press to form the austenitized blank;

[0100] Based on the servo press, the pressure on the die is maintained, and the formed blank is subjected to zoned temperature-controlled quenching;

[0101] The pressure of the servo press is unloaded, the blank after zone temperature-controlled quenching is taken out, and trimming and punching are performed to obtain the target component.

[0102] In the above process, the outside of the mold can be heated uniformly without modifying the mold's cooling pipeline and other structures. The mold gap and the thermal insulation coating are used to achieve zoned temperature-controlled quenching of the formed blank.

[0103] The present invention also provides a preferred embodiment, so that the final integrated complex component has higher strength and better collision performance:

[0104] The blank thickness of the hard zone is 1.0mm-2.0mm, and the target strength of the hard zone is tensile strength, which ranges from 1300MPa to 2000MPa; the blank thickness of the transition zone is 1.0mm-2.0mm, and the target strength of the transition zone is tensile strength, which ranges from 1000MPa to 1300MPa; the blank thickness of the soft zone is 1.0mm-2.0mm, and the target strength of the soft zone is tensile strength, which ranges from 600MPa to 1200MPa; the blanks are connected by laser welding, the welding current of the laser welding is 50A-300A, the laser pulse frequency is 20Hz-50Hz, the laser pulse width is 2.5ms-5.0ms, and the welding speed is 100mm / min-370mm / min;

[0105] The thickness of the patch plate is 1.0 mm-2.0 mm, the tensile strength of the patch plate is 1300 MPa-2000 MPa, and the patch plate is connected to the blank by spot welding;

[0106] The material of the thermal insulation coating is high-temperature reflective thermal insulation nano-composite ceramic coating GN-302A. When applying the thermal insulation coating, the first natural drying time is 20min-40min, the first baking temperature is 400℃-700℃, and the first baking time is 20min-40min; the high-temperature sealing reinforcing agent is F2A, the second natural drying time is 10min-30min, the second baking temperature is 250℃-300℃, and the second baking time is 10min-30min;

[0107] The heating temperature of the heating furnace is 900℃-950℃, and the holding time is 3min-5min; the time for transferring and positioning the billet on the mold is 3s-8s; the temperature of the mold is 20℃-150℃, and the mold gap is 0mm-0.2mm; the pressure on the mold is maintained at 1000KN-3500KN, and the zone temperature control quenching time is 5s-20s.

[0108] The present invention also provides a more detailed embodiment to more clearly illustrate the above steps S101 to S105:

[0109] (1) Material selection and partition design: In this embodiment, the target component is an integrated door ring, and its partition diagram is as follows: Figure 3 and Figure 4 As shown, the door ring is made of ultra-high strength steel B1500HS. The A-pillar of the door ring is formed by connecting the A-pillar lower section 1 and the A-pillar upper section 2, and the B-pillar is formed by connecting the B-pillar upper section 3 and the B-pillar lower section-rear door sill 4, wherein the B-pillar lower section and the rear door sill are made of the same blank. The upper section 2 of the A-pillar and the upper section 3 of the B-pillar are set as hard areas with a tensile strength of 1500MPa, the upper section 2 of the A-pillar is 1.5mm thick, and the upper section 3 of the B-pillar is 1.8mm thick; the lower section of the B-pillar-rear door sill 4 is set as a soft area with a tensile strength of 1000MPa and a material thickness of 1.5mm; the lower section of the A-pillar 1 and the front door sill 5 are set as transition areas with a strength between the soft area and the hard area and a tensile strength of 1300MPa, the lower section of the A-pillar 1 is 1.3mm thick, and the front door sill 5 is 1.4mm thick; the upper section of the A-pillar patch plate 6 has a tensile strength of 1500MPa and a material thickness of 1.2mm; the upper section of the B-pillar patch plate 7 has a tensile strength of 1500MPa and a material thickness of 1.5mm.

[0110] There are five welds, namely a first weld 11 , a second weld 12 , a third weld 13 , a fourth weld 14 and a fifth weld 15 .

[0111] (2) Patch board design and solder joint arrangement:

[0112] The outer ring size of the A-pillar upper patch plate 6 is 400×200, the ring width △d=100, the spacing between the inner ring welding points is 32, 64, 96…, the spacing between the outer ring welding points is 40, 80, 120…, all in mm; the outer ring size of the B-pillar upper patch plate 7 is 700×150, the ring width △d=80, the spacing between the inner ring welding points is 20, 40, 60…, the spacing between the outer ring welding points is 30, 60, 90…, all in mm. The schematic diagram of the welding points of the patch plate is as follows Figure 5 shown.

[0113] (3) Relationship image acquisition:

[0114] Effect of heat transfer coefficient on tensile strength of B1500HS steel plate Figure 6 When HTC≤500W / m 2 K, the tensile strength increases significantly with the increase of HTC. When HTC≥600W / m 2 K, the tensile strength is above 1400MPa.

[0115] Effect of die gap on tensile strength of B1500HS steel plate Figure 7 As shown, when the heat transfer coefficient is 300W / m 2 K and 400W / m 2 K, the tensile strength decreases with the increase of die gap.

[0116] (4) Selection of hot forming process parameters:

[0117] The optimal process parameter combination for hot forming of tailor-made welded door rings obtained based on response surface methodology-multi-objective optimization genetic algorithm is forming temperature T=850℃, friction coefficient μ=0.18, and forming speed v=181.8mm / s.

[0118] (5) Combination Figure 8 As shown in the figure, the actual curve development is carried out using the servo press multi-point free programming mode, and the mixed-order servo control curve (i.e., servo process curve) is obtained as follows:

[0119]

[0120] (6) Door ring zone temperature control quenching process:

[0121] According to the strength requirements of each area of ​​the door ring in (1) and the relationship diagram in (3), the mold gap and heat transfer coefficient are determined. The gap between the mold and the blank is changed, and a thermal insulation coating with a thickness corresponding to the heat transfer coefficient is applied to change the heat transfer coefficient between each area of ​​the blank and the mold. By controlling the cooling rate of the blank in each area during the forming process, zoned temperature controlled quenching is achieved, achieving the purpose of accurately controlling the microstructure and properties of ultra-high strength steel.

[0122] In this embodiment, the mold temperature is controlled at 20°C-100°C.

[0123] The door ring hard area (A-pillar upper section 2 and B-pillar upper section 3) blanks are not coated, so that the HTC between the hard area blanks and the mold is ≥2000W / m 2 K, during the pressure-holding quenching process, the cooling rate of the hard zone blank during the partition quenching process is ≥ the critical cooling rate of martensite to ensure the formation of full martensite structure;

[0124] The transition area (A-pillar lower section 1, A-pillar upper section 2 and front door sill 5) is coated with GN-302A thermal insulation coating with a thickness of 0.02mm-0.05mm, so that the heat transfer coefficient between the blank and the mold is 400W / m 2 K-500W / m 2 K, during the partition quenching process, the cooling rate of the soft zone billet is less than the critical cooling rate of martensite, and a martensite-bainite composite structure is generated;

[0125] The mold gap of the door ring soft area (lower section of B pillar-rear door sill 4) is 0.15mm, and the soft area blank is coated with GN-302A thermal insulation coating with a thickness of 0.06mm-0.10mm, so that the heat transfer coefficient between the blank and the mold is 300W / m 2 K-400W / m 2 K, during the partition quenching process, the cooling rate of the soft zone billet is less than the critical cooling rate of martensite, and a martensite-bainite composite structure is generated.

[0126] (7) Method for manufacturing door ring: Based on the above (1), (2), (3), (4), (5) and (6), a one-piece door ring variable strength hot stamping forming process is developed, the method comprising the following steps:

[0127] S1. Cutting: Determine the size of the blank according to the structural sizes of the A-pillar lower section 1, the A-pillar upper section 2, the B-pillar upper section 3, the B-pillar lower section-rear door sill 4 and the front door sill 5.

[0128] S2. Blank connection: The A-pillar lower section 1, the A-pillar upper section 2, the B-pillar upper section 3, the B-pillar lower section-rear door sill 4 and the front door sill 5 are laser welded end to end in sequence to form an integrated door ring blank; the A-pillar upper section patch plate 6 and the B-pillar upper section patch plate 7 are respectively connected to the door ring blank with variable spacing welding points.

[0129] The laser welding process parameters are as follows: welding current is 150A, frequency is 20Hz, pulse width is 4.5ms, and welding speed is 360mm / min. The inner ring welding point spacings of the A-pillar upper patch plate 6 are 32mm, 64mm, 96mm, and 128mm, respectively, and the outer ring welding point spacings are 40mm, 80mm, 120mm, and 160mm, respectively; the inner ring welding point spacings of the B-pillar upper patch plate 7 are 20mm, 40mm, 60mm, and 80mm, respectively, and the outer ring welding point spacings are 30mm, 60mm, 90mm, and 120mm, respectively.

[0130] S3. Coating the blank with thermal insulation coating: Evenly coat the ceramic thermal insulation coating on both sides of the blank in the soft zone and transition zone. After natural drying, put it into a heating furnace and bake it until the coating is completely dry. Take out the blank, cool it to room temperature and spray it with high-temperature sealing enhancer F2A. After natural drying, put it into a heating furnace and bake it until it is completely dry. This completes one coat.

[0131] The transition zone is coated once, the natural drying time of the heat insulation layer is 20 minutes, the baking temperature of the heat insulation layer is 500°C, the baking time of the heat insulation layer is 30 minutes, the natural drying time of the sealing reinforcement layer is 10 minutes, the baking temperature of the sealing reinforcement layer is 250°C, and the baking time of the sealing reinforcement layer is 15 minutes.

[0132] The soft area is coated twice, the natural drying time of the heat insulation layer is 20 minutes, the baking temperature of the heat insulation layer is 500°C, the baking time of the heat insulation layer is 30 minutes, the natural drying time of the sealing reinforcement layer is 10 minutes, the baking temperature of the sealing reinforcement layer is 250°C, and the baking time of the sealing reinforcement layer is 15 minutes. The above steps are repeated twice.

[0133] The hard zone blank is not subjected to coating treatment; the coating thickness of the transition zone blank is 0.04 mm; and the coating thickness of the soft zone blank is 0.08 mm.

[0134] S4. Servo process curve input: input the servo process curve into the servo hot stamping process intelligent design system.

[0135] S5. Heating for austenitization: The blank is transferred to a heating furnace and heated to 900°C and kept at this temperature for 5 minutes to achieve complete austenitization.

[0136] S6, transfer: Use a robot to take the door ring blank out of the heating furnace, transfer it and position it on the mold. The transfer time is 5s.

[0137] S7, mold closing and forming: the upper mold moves downward, and the door ring blank begins to be formed by servo speed change until the upper and lower molds are closed, the mold gap is 0.15mm, and the forming is completed.

[0138] The forming temperature is 850° C., and the friction coefficient between the blank and the die is 0.18.

[0139] S8, zone quenching: The high temperature reflective insulation nano-composite ceramic coating GN-302A coated on the surface of the blank changes the heat transfer coefficient between the blank and the mold, and realizes the zone temperature controlled quenching of the door ring through the mold gap / variable coating thickness. The overall door ring mold temperature is 20℃-100℃. The pressure of the zone quenching is 2000KN, and the holding time is 10s.

[0140] S9, trimming and punching: the press is unloaded, the upper die moves upward, the formed part is taken out by a robot, and laser cutting is used to trim and punch the edges, and finally the door knocker is obtained.

[0141] According to the manufacturing method of the door ring, the door ring welding integral hot stamping-partition quenching integrated forming simulation was carried out, and the maximum thinning rate was 20.9%, and the maximum springback after trimming was 0.82mm. The forming quality was good, and the strength met the design requirements of the door ring. Fig. 9 This is a cloud diagram of the tensile strength distribution of the door knocker finally obtained in this embodiment.

[0142] The beneficial effects of this embodiment are:

[0143] 1. Hot forming integrated complex components, simple forming process and high production efficiency;

[0144] 2. The door ring blank is formed by laser welding, and the blank is made of the same material to avoid cracking of the weld caused by the difference in organization and mechanical properties at both ends of the weld, and the weld performance is stable;

[0145] 3. Design an annular patch plate to simultaneously improve local stiffness and lightweight levels;

[0146] 4. Connect the patch plate and the door ring blank through variable spacing welding points to increase the connection strength and fatigue resistance;

[0147] 5. Design servo hot forming process curve, dynamically adjust deformation speed, and improve forming performance;

[0148] 6. Develop a hot stamping process for integrated complex components, accurately control the microstructure and properties of ultra-high-strength steel, match the strength and toughness of the door ring, and meet collision requirements.

[0149] Furthermore, the present invention also provides an integrated complex component, which is manufactured by the method of any of the above embodiments. The advantages of the complex component have been described in detail above, so it will not be explained in detail in this article.

[0150] The present invention provides a servo hot forming and partition quenching method for an integrated complex component and a component. First, the design information of a target component is obtained, the target component includes a plurality of partitions, the design information includes the manufacturing material of the target component, and then the heat transfer coefficient and mold gap corresponding to each partition are obtained according to the manufacturing material. Then, the thickness of the thermal insulation coating corresponding to each partition is obtained according to the heat transfer coefficient. Then, a blank is manufactured according to the design information, and a thermal insulation coating is coated on the surface of each partition based on the thickness of the thermal insulation coating corresponding to each partition. Finally, a mold is manufactured according to the mold gap corresponding to each partition, the blank is servo hot formed by the mold, and partition quenching is performed based on the thermal insulation coating thickness corresponding to the surface of each partition and the heat transfer coefficient, so as to obtain the formed target component. Compared with the prior art, the present invention changes the heat transfer coefficient between each area of ​​the blank and the mold by applying a thermal insulation coating with a thickness corresponding to the heat transfer coefficient, and at the same time cooperates with different mold spacings between the mold and the blank. At the same time, the formability of the one-piece complex component is improved through a servo hot forming process, and the cooling rate of the blank in each area during the forming process is controlled, thereby realizing zoned temperature controlled quenching and achieving the purpose of adjusting local mechanical properties, so that the manufactured one-piece complex component has both sufficient strength and good collision performance.

[0151] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for servo hot forming partition quenching of an integrated complex component, characterized in that: include: Acquire design information of a target component, the target component comprising a plurality of partitions, the design information comprising a manufacturing material of the target component; According to the manufacturing material, a heat transfer coefficient and a mold gap corresponding to each partition are obtained; According to the heat transfer coefficient, the thickness of the thermal insulation coating corresponding to each partition is obtained; Manufacturing a blank according to the design information, and coating a thermal insulation coating on the surface of each partition based on the thickness of the thermal insulation coating corresponding to each partition; A mold is manufactured according to the mold gap corresponding to each partition, the blank is servo hot-formed by the mold, and a thermal insulation coating with a thickness corresponding to the heat transfer coefficient on the surface of each partition is subjected to partition quenching to obtain the formed target component; A patch plate is welded to the partition where the position to be strengthened in the target component is located, the patch plate is annular, and the welding points between the patch plate and the target component are arranged with variable spacing; The multiple subareas include a hard area, a transition area, and a soft area, the target intensity of the hard area is greater than the target intensity of the transition area, and the target intensity of the transition area is greater than the target intensity of the soft area; The hard zone is welded to connect the patch plate; the thickness of the thermal insulation coating is inversely proportional to the target strength; The method of manufacturing a blank according to the design information and coating the thermal insulation coating on the surface of each partition based on the thickness of the thermal insulation coating corresponding to each partition comprises: Manufacturing the blank according to the design information, and welding the patch plate to the blank; Based on the thickness of the thermal insulation coating corresponding to each partition, respectively apply the thermal insulation coating on the surface of each partition of the blank; Allowing the blank coated with the heat-insulating coating to dry naturally for the first time, and then baking it for the first time; Stop the first baking, and after the blank is cooled to room temperature, spray a high-temperature sealing reinforcing agent on the outside of the thermal insulation coating; Allowing the blank coated with the high-temperature sealing reinforcing agent to dry naturally for a second time, and then baking it for a second time; The design information also includes a target strength of each partition; and the heat transfer coefficient and mold gap corresponding to each partition are obtained according to the manufacturing material, including: According to the manufacturing material, a heat transfer coefficient-strength performance relationship diagram and a mold gap-strength performance relationship diagram of the manufacturing material are obtained; According to the target strength of each partition, based on the heat transfer coefficient-strength performance relationship diagram, the heat transfer coefficient corresponding to each partition is obtained; According to the target strength of each partition, based on the mold gap-strength performance relationship diagram, the mold gap corresponding to each partition is obtained.

2. The integrated complex component servo hot forming zone quenching method according to claim 1 is characterized in that: The method comprises: manufacturing a mold according to the mold gap corresponding to each partition, performing servo hot forming on the blank through the mold, and performing partition quenching based on the thickness of the thermal insulation coating corresponding to the heat transfer coefficient on the surface of each partition to obtain the formed target component, including: The mold is manufactured according to the mold gap corresponding to each partition; Setting initial hot forming process parameters, and optimizing the initial hot forming process parameters based on a genetic algorithm to obtain target hot forming process parameters; According to the target hot forming process parameters, a servo process curve is obtained; According to the servo process curve, the blank is subjected to servo hot forming through the die, and partition quenching is performed on the thermal insulation coating with a thickness corresponding to the heat transfer coefficient on each partition surface to obtain the formed target component.

3. The integrated complex component servo hot forming zone quenching method according to claim 2 is characterized in that: The servo process curve includes: S ( t ) = αt 3 +β t 2 + γt + η in, S ( t ) is the displacement of the pressure head in the servo press, t For time, α , β, γ and η for different adjustment factors.

4. The integrated complex component servo hot forming zone quenching method according to claim 2 is characterized in that: According to the servo process curve, the blank is subjected to servo hot forming by the die, and a thermal insulation coating having a thickness corresponding to a heat transfer coefficient on each partition surface is subjected to partition quenching to obtain the formed target component, comprising: The billet is heated and kept warm in a heating furnace to be completely austenitized; Transfer and position the austenitized billet onto the die; According to the servo process curve, the mold is closed based on a servo press to form the austenitized blank; Based on the servo press, the pressure is maintained continuously and the formed blank is subjected to zoned temperature-controlled quenching; The pressure of the servo press is unloaded, the blank after zone temperature-controlled quenching is taken out, and trimming and punching are performed to obtain the target component.

5. The integrated complex component servo hot forming zone quenching method according to claim 4 is characterized in that: In the target component, the blank thickness of the hard zone is 1.0mm-2.0mm, and the target strength of the hard zone is tensile strength, which ranges from 1300MPa to 2000MPa; the blank thickness of the transition zone is 1.0mm-2.0mm, and the target strength of the transition zone is tensile strength, which ranges from 1000MPa to 1300MPa; the blank thickness of the soft zone is 1.0mm-2.0mm, and the target strength of the soft zone is tensile strength, which ranges from 600MPa to 1200MPa; the blanks are connected by laser welding, the welding current of the laser welding is 50A-300A, the laser pulse frequency is 20Hz-50Hz, the laser pulse width is 2.5ms-5.0ms, and the welding speed is 100mm / min-370mm / min; The thickness of the patch plate is 1.0 mm-2.0 mm, the tensile strength of the patch plate is 1300 MPa-2000 MPa, and the patch plate is connected to the blank by spot welding; The material of the thermal insulation coating is high-temperature reflective thermal insulation nano-composite ceramic coating GN-302A. When applying the thermal insulation coating, the first natural drying time is 20min-40min, the first baking temperature is 400℃-700℃, and the first baking time is 20min-40min; the high-temperature sealing reinforcing agent is F2A, the second natural drying time is 10min-30min, the second baking temperature is 250℃-300℃, and the second baking time is 10min-30min; The heating temperature of the heating furnace is 900℃-950℃, and the holding time is 3min-5min; the time for transferring and positioning the billet on the mold is 3s-8s; the temperature of the mold is 20℃-150℃, and the mold gap is 0mm-0.2mm; the pressure on the mold is maintained at 1000kN-3500kN, and the zone temperature control quenching time is 5s-20s.

6. An integrated complex component, characterized in that: The integrated complex component is manufactured by the servo hot forming and zone quenching method described in any one of claims 1 to 5.