A composite coating material containing mussel byssus protein and preparation method thereof

By preparing TiO2 and Ag layers on the surface of carbon steel and spin-coated Mefp-1 protein solution to form Mefp-1/TiO2/Ag composite coating, the problem of insufficient use of harmful chemicals and anti-corrosion and wear resistance in the prior art is solved. , achieving environmentally friendly, multi-functional efficient anti-corrosion and wear resistance.

CN117568758BActive Publication Date: 2024-11-15CHINA UNIV OF MINING & TECH (BEIJING)
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202311285578.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-07
Publication Date
2024-11-15
Estimated Expiration
2043-10-07

AI Technical Summary

Technical Problem

The existing carbon steel anti-corrosion coating materials use harmful chemicals, which pollute the environment and cause harm to the human body, and it is difficult to meet the anti-corrosion and wear resistance requirements under harsh working conditions.

Method used

TiO2 and Ag layers were prepared by DC magnetron sputtering, and spin-coated Mefp-1 protein solution on the basis to form Mefp-1/TiO2/Ag composite coating, which was used to enhance the strong adhesion and cohesion properties of Mefp-1 protein. Adhesion and protection of the coating.

Benefits of technology

It realizes an environmentally friendly multi-function coating, significantly improves the corrosion and wear resistance of carbon steel, enhances the adhesion and protection of magnetron sputtering coating, and reduces cost and operational complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004479705280000061
    Figure BDA0004479705280000061
  • Figure BDA0004479705280000072
    Figure BDA0004479705280000072
  • Figure BDA0004479705280000073
    Figure BDA0004479705280000073
Patent Text Reader

Abstract

The invention discloses a composite coating material containing mussel foot silk protein and a preparation method thereof, the surface of carbon steel is cleaned to remove the surface oxide film; a TiO2 layer is prepared on the surface of carbon steel by DC magnetron sputtering; an Ag layer is prepared on the surface of carbon steel by DC magnetron sputtering; a TiO2 / Ag film contained on the surface of carbon steel is used as a precursor film, and a layer of Mefp-1 protein solution is spin-coated on the precursor film by a homogenizer to obtain a Mefp-1 / TiO2 / Ag composite coating for the surface of carbon steel. The TiO2 coating mainly plays an anti-corrosion role, and the Ag coating has excellent wear resistance. Both coatings belong to environmentally friendly materials in the field of anti-corrosion and wear resistance, and are used to replace harmful chemicals. Mefp-1 protein has a certain effect on improving the anti-corrosion and wear resistance of carbon steel, and greatly enhances the adhesion of magnetron sputtering coatings, so that the protective performance of magnetron sputtering coatings is doubled. The present invention can effectively improve the corrosion resistance and wear resistance of carbon steel, and also has the advantages of simple operation and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating materials, and in particular to a composite coating material containing mussel byssus protein and a preparation method thereof. Background Art

[0002] Carbon steel is one of the most widely used metals in industrial production. Due to its poor corrosion resistance and wear resistance, it causes huge economic losses every year. Traditional carbon steel anti-corrosion coatings use a large amount of harmful chemicals, such as chromates, heavy metals and volatile organic compounds, which not only seriously pollute the environment, but also cause irreversible harm to the human body. In order to reduce the wear and failure of carbon steel, the industry usually adopts methods such as adding lubricants or grease to reduce friction, but the large amount of waste oil generated during use is difficult to handle. If not handled properly, it will cause serious damage to the ecosystem. Therefore, it has become very necessary to develop a multifunctional environmentally friendly coating that has anti-corrosion, friction reduction and wear resistance.

[0003] CN109468601A discloses a method for magnetron sputtering deposition of amorphous tantalum coating on the surface of carbon steel, the steps of which are: mechanically grinding and polishing the sample with sandpaper, and ultrasonic cleaning; fixing the sample on the sputtering platform of ultra-high vacuum magnetron sputtering equipment, placing the target material in the magnetron sputtering chamber, closing the sputtering chamber, and evacuating to a certain background vacuum; using a DC magnetron sputtering method to prepare an amorphous tantalum coating. Magnetron sputtering coating has the advantages of good uniformity, good density, and strong adhesion, and is widely used to improve the corrosion resistance and wear resistance of carbon steel. However, the thickness of the coating prepared by magnetron sputtering technology is only at the micron level. In the face of harsh working conditions, it is difficult to meet the requirements by relying solely on magnetron sputtering coatings, and it is necessary to combine other technical means to further improve the physical properties of the coating to achieve better corrosion resistance and wear resistance. Summary of the invention

[0004] The purpose of the present invention is to provide a composite coating material containing mussel byssus protein and a preparation method thereof, so as to solve the problem that the existing coating materials are unfriendly to the environment and human body.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solution: a method for preparing a composite coating material containing mussel byssin, characterized in that the steps are as follows:

[0006] S1. Clean the surface of carbon steel and remove the surface oxide film;

[0007] S2. Preparation of TiO2 layer on carbon steel surface by DC magnetron sputtering;

[0008] S3. Prepare Ag layer on carbon steel surface by DC magnetron sputtering;

[0009] S4. Using the TiO2 / Ag film contained on the surface of carbon steel as a precursor film, a layer of Mefp-1 protein solution is spin-coated on the precursor film using a homogenizer to obtain a Mefp-1 / TiO2 / Ag composite coating for the surface of carbon steel.

[0010] A further technical solution is that step S1 specifically comprises the following steps: grinding the surface of the carbon steel substrate with water sandpaper, and then polishing it with diamond polishing paste and real velvet polishing cloth, wherein the surface roughness Ra is less than 0.3 μm after polishing, and the surface oxide film is removed; then the carbon steel substrate is rinsed with deionized water, placed in anhydrous ethanol and cleaned with ultrasonic wave, and then taken out and rinsed with deionized water and blown dry for use.

[0011] A further technical solution is that step S2 specifically selects a Ti target with a purity of 99.99%, places the treated carbon steel in the center of the sputtering table of the magnetron sputtering equipment, keeps a constant distance between the target and the substrate, introduces argon and oxygen, the magnetron sputtering power is 80 to 120 W, and the magnetron sputtering time is 40 to 80 min.

[0012] A further technical solution is that the target material is sputtered and cleaned in a pure argon environment of 10Pa for 10 minutes before deposition, the distance is constant at 5cm, the speed of the sputtering table is set to 3rpm, and after sputtering is completed, it is kept in the vacuum chamber for 20 minutes.

[0013] A further technical solution is that step S3 specifically selects an Ag target material with a purity of 99.99%. Before deposition, the target material is sputtered and cleaned in a pure argon environment of 10Pa for 10 minutes, argon is introduced, the magnetron sputtering power is 50-90W, and the magnetron sputtering time is 5-30 minutes.

[0014] A further technical solution is that the introduction rate of argon gas during the sputtering process is 10 to 30 ml / min.

[0015] A further technical solution is that the Mefp-1 protein solution in step S4 is based on Mefp-1 protein and diluted with citric acid solution, with a pH value of 5 to 9 and a concentration of 0.05 to 0.2 mg / mL.

[0016] A further technical solution is that in step S4, the glue homogenizer first performs low-speed spin coating and then high-speed spin coating, the low-speed spin coating speed is 500-1000rpm, the low-speed spin coating time is 10-30s, and the high-speed spin coating speed is 2000-4000rpm, and the high-speed spin coating time is 50-70s.

[0017] A further technical solution is a composite coating material containing mussel byssus protein prepared by the above method.

[0018] Working mechanism: This is because the TiO2 coating is dense and stable, and it adheres tightly to the carbon steel surface to form a protective barrier. In addition, the chemical properties of TiO2 itself are stable and it is not easy to react with other substances, so that carbon steel covered with TiO2 coating can effectively resist corrosion in salt water and some acidic environments. The excellent ductility of the Ag coating allows the silver coating to undergo plastic shear between the relative sliding surfaces, thereby playing a lubricating role. Mefp-1 protein, a natural protein derived from marine mussels, is a green and environmentally friendly natural material with extremely strong adhesion and cohesion properties. Its super strong adhesion and cohesion properties come from the large amount of di-hydroxyphenylalanine (DOPA) it contains. DOPA can react with the prepared TiO2 coating or Ag coating to further enhance the adsorption of the magnetron sputtering coating on the metal surface. When carbon steel generates oxides due to corrosion, DOPA can also react with the generated oxides to form a denser protective layer, thereby preventing the further progress of the corrosion reaction.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: in the Mefp-1 / TiO2 / Ag composite coating material prepared by the present invention, the TiO2 coating mainly plays an anti-corrosion role, and the Ag coating has excellent wear resistance. Both coatings are environmentally friendly materials in the field of corrosion resistance and wear resistance, and are used to replace harmful chemicals. Mefp-1 protein has a certain effect on improving the corrosion resistance and wear resistance of carbon steel. More importantly, the addition of Mefp-1 protein can greatly enhance the adhesion of the magnetron sputtering coating and multiply the protective performance of the magnetron sputtering coating. On the premise of being able to effectively improve the corrosion resistance and wear resistance of carbon steel, the present invention also has the advantages of simple operation and low cost, and can provide a reference for the industrial application of mussel foot silk protein in the direction of corrosion resistance and wear resistance of carbon steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 (a) is the carbon steel surface after pretreatment, and (b) is the surface covered with Mefp-1 / TiO2 / Ag composite coating.

[0021] Figure 2 (a) is the nano scratch test result of TiO2 coating, (b) is the nano scratch test result of TiO2 / Ag coating, and (c) is the nano scratch test result of Example 1.

[0022] Figure 3 The friction coefficient variation curves of Example 1, carbon steel sample, TiO2 coating sample, and TiO2 / Ag coating sample over time.

[0023] Figure 4The curves showing the change of polarization resistance of the carbon steel sample, the TiO2 coating sample and the TiO2 / Ag coating sample with immersion time are shown in Example 1. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0025] Example 1

[0026] Step 1: Select a Q235 carbon steel sheet with a diameter of 15mm and a thickness of 2mm, and grind the sample with water sandpaper 400#, 800#, and 1200# in turn, and then polish it with w2.5 diamond polishing paste and real velvet polishing cloth to remove the oxide film on the surface. Rinse the sample with deionized water and put it into anhydrous ethanol for ultrasonic cleaning for 8 minutes. After taking it out, rinse it with deionized water and blow it dry to obtain the pretreated Q235 carbon steel sample for standby use.

[0027] Figure 1 (a) is the microscopic morphology of the carbon steel surface after treatment. It can be seen that there are a few wear marks left on the surface of the treated carbon steel during the grinding process, but the surface is basically flat.

[0028] Step 2: Place the sample in the center of the sputtering table of the magnetron sputtering equipment. The distance between the target and the substrate is constant at 5 cm, and the sputtering table speed is set to 3 rpm. A Ti target with a purity of 99.99% is selected. Before deposition, the target is sputtered and cleaned in a pure argon environment of 10 Pa for 10 minutes. Then oxygen and argon are introduced in a ratio of 2:10. The sputtering power is set to 100w and the sputtering time is 60 minutes. After sputtering, continue to keep it in the vacuum chamber for 20 minutes.

[0029] Step 3: Place the sample in the center of the sputtering table of the magnetron sputtering equipment. The distance between the target and the substrate is constant at 5 cm, and the sputtering table speed is set to 3 rpm. Select an Ag target with a purity of 99.99%. Before deposition, the target is sputtered and cleaned in a pure argon environment of 10 Pa for 10 minutes. Then, argon is introduced at a rate of 20 mL / min. The sputtering power is set to 70w, and the sputtering time is 10 minutes. After sputtering, continue to keep it in the vacuum chamber for 20 minutes.

[0030] Step 4: Select Mefp-1 protein with a content of 1 mg / ml and a purity of 92%, and dilute the solution to 0.1 mg / ml with 1 wt.% citric acid. Adjust the pH value to 7 with saturated KOH. Take a small amount of the prepared solution and drop it onto the surface of the sample. Spin it on a homogenizer at 700 rpm for 20 seconds and 3000 rpm for 60 seconds. The Mefp-1 / TiO2 / Ag composite coating is obtained, which is recorded as (MTA-1).

[0031] Figure 1 (b) is a microscopic observation picture of the obtained Mefp-1 / TiO2 / Ag coating. The obtained composite coating is uniform, dense, and relatively flat without obvious defects.

[0032] like Figure 3 As shown in the figure, the friction coefficient curves of the Mefp-1 / TiO2 / Ag composite coating obtained in this example, the TiO2 / Ag coating of Comparative Example 2, the TiO2 coating of Comparative Example 1, and the carbon steel sample under dry friction conditions at room temperature. It can be seen that the tribological performance of the Mefp-1 / TiO2 / Ag composite coating is much better than that of other coatings.

[0033] like Figure 4 As shown in the figure, during the long immersion process, the polarization resistance of this example gradually increases with the increase of immersion time, and finally is much higher than the polarization resistance of carbon steel. This shows that with the increase of immersion time, the anti-corrosion performance of the coating is significantly improved.

[0034] Example 2

[0035] Step 1: Select a Q235 carbon steel sheet with a diameter of 15mm and a thickness of 2mm, and use water sandpaper 400#, 800#, and 1200# to polish the sample in turn. Then polish with w2.5 diamond polishing paste and real velvet polishing cloth to remove the oxide film on the surface. Rinse the sample with deionized water and put it into anhydrous ethanol for ultrasonic cleaning for 8 minutes. After taking it out, rinse it with deionized water and blow it dry to obtain the pretreated Q235 carbon steel sample for use.

[0036] Step 2: Place the sample in the center of the sputtering table of the magnetron sputtering equipment. The distance between the target and the substrate is constant at 5 cm, and the sputtering table speed is set to 3 rpm. A Ti target with a purity of 99.99% is selected. Before deposition, the target is sputtered and cleaned in a pure argon environment of 10 Pa for 10 minutes. Then oxygen and argon are introduced in a ratio of 2:10. The sputtering power is set to 100w and the sputtering time is 80 minutes. After sputtering, continue to keep it in the vacuum chamber for 20 minutes.

[0037] Step 3: Place the sample in the center of the sputtering table of the magnetron sputtering equipment. The distance between the target and the substrate is constant at 5 cm, and the sputtering table speed is set to 3 rpm. Select an Ag target with a purity of 99.99%. Before deposition, the target is sputtered and cleaned in a pure argon environment of 10 Pa for 10 minutes. Then argon is introduced at a rate of 20 mL / min. The sputtering power is set to 70w and the sputtering time is 20 minutes. After sputtering, continue to keep it in the vacuum chamber for 20 minutes.

[0038] Step 4: Select Mefp-1 protein with a content of 1 mg / ml and a purity of 92%, and dilute the solution to 0.1 mg / ml with 1 wt.% citric acid. Adjust the pH value to 7 with saturated KOH. Take a small amount of the prepared solution and drop it onto the sample surface. Spin it on a homogenizer at 700 rpm for 20 seconds and 3000 rpm for 60 seconds. The Mefp-1 / TiO2 / Ag composite coating (referred to as MTA-2) is obtained.

[0039] Example 3

[0040] Step 1: Select a Q235 carbon steel sheet with a diameter of 15mm and a thickness of 2mm, and use water sandpaper 400#, 800#, and 1200# to polish the sample in turn. Then polish with w2.5 diamond polishing paste and real velvet polishing cloth to remove the oxide film on the surface. Rinse the sample with deionized water and put it into anhydrous ethanol for ultrasonic cleaning for 8 minutes. After taking it out, rinse it with deionized water and blow it dry to obtain the pretreated Q235 carbon steel sample for use.

[0041] Step 2: Place the sample in the center of the sputtering table of the magnetron sputtering equipment. The distance between the target and the substrate is constant at 5 cm, and the sputtering table speed is set to 3 rpm. A Ti target with a purity of 99.99% is selected. Before deposition, the target is sputtered and cleaned in a pure argon environment of 10 Pa for 10 minutes. Then oxygen and argon are introduced in a ratio of 2:10. The sputtering power is set to 100w and the sputtering time is 60 minutes. After sputtering, continue to keep it in the vacuum chamber for 20 minutes.

[0042] Step 3: Place the sample in the center of the sputtering table of the magnetron sputtering equipment. The distance between the target and the substrate is constant at 5 cm, and the sputtering table speed is set to 3 rpm. Select an Ag target with a purity of 99.99%. Before deposition, the target is sputtered and cleaned in a pure argon environment of 10 Pa for 10 minutes. Then, argon is introduced at a rate of 20 mL / min. The sputtering power is set to 70w, and the sputtering time is 10 minutes. After sputtering, continue to keep it in the vacuum chamber for 20 minutes.

[0043] Step 4: Select Mefp-1 protein with a content of 1 mg / ml and a purity of 92%, and dilute the solution to 0.1 mg / ml with 1 wt.% citric acid. Adjust the pH value to 7 with saturated KOH. Take a small amount of the prepared solution and drop it onto the surface of the sample. Spin it on a homogenizer at 1000 rpm for 20 seconds and 4000 rpm for 60 seconds. The Mefp-1 / TiO2 / Ag composite coating is obtained, which is recorded as MTA-3.

[0044] Example 4

[0045] Step 1: Select a Q235 carbon steel sheet with a diameter of 15mm and a thickness of 2mm, and use water sandpaper 400#, 800#, and 1200# to polish the sample in turn. Then polish with w2.5 diamond polishing paste and real velvet polishing cloth to remove the oxide film on the surface. Rinse the sample with deionized water and put it into anhydrous ethanol for ultrasonic cleaning for 8 minutes. After taking it out, rinse it with deionized water and blow it dry to obtain the pretreated Q235 carbon steel sample for use.

[0046] Step 2: Place the sample in the center of the sputtering table of the magnetron sputtering equipment. The distance between the target and the substrate is constant at 5 cm, and the sputtering table speed is set to 3 rpm. A Ti target with a purity of 99.99% is selected. Before deposition, the target is sputtered and cleaned in a pure argon environment of 10 Pa for 10 minutes. Then oxygen and argon are introduced in a ratio of 2:10. The sputtering power is set to 100w and the sputtering time is 60 minutes. After sputtering, continue to keep it in the vacuum chamber for 20 minutes.

[0047] Step 3: Place the sample in the center of the sputtering table of the magnetron sputtering equipment. The distance between the target and the substrate is constant at 5 cm, and the sputtering table speed is set to 3 rpm. Select an Ag target with a purity of 99.99%. Before deposition, the target is sputtered and cleaned in a pure argon environment of 10 Pa for 10 minutes. Then, argon is introduced at a rate of 20 mL / min. The sputtering power is set to 70w, and the sputtering time is 10 minutes. After sputtering, continue to keep it in the vacuum chamber for 20 minutes.

[0048] Step 4: Select Mefp-1 protein with a content of 1 mg / ml and a purity of 92%, and dilute the solution to 0.1 mg / ml with 1wt.% citric acid. Adjust the pH value to 7 with saturated KOH. Take a small amount of the prepared solution and drop it onto the sample surface. Spin it on a gel coater at 500 rpm for 20 seconds and 2000 rpm for 60 seconds. The Mefp-1 / TiO2 / Ag composite coating is obtained. (Recorded as MTA-4)

[0049] Comparative Example 1

[0050] A Q235 carbon steel sheet with a diameter of 15 mm and a thickness of 2 mm was selected, and the samples were polished in turn using water sandpaper 400#, 800#, and 1200#. Then, the samples were polished with w2.5 diamond polishing paste and real velvet polishing cloth to remove the oxide film on the surface. The samples were rinsed with deionized water and then placed in anhydrous ethanol for ultrasonic cleaning for 8 minutes. After being taken out, they were rinsed with deionized water and blown dry to obtain the pretreated Q235 carbon steel sample (referred to as BC-1).

[0051] Comparative Example 2

[0052] The same as Example 1, except that only steps 1 and 2 are performed.

[0053] The specific steps are as follows:

[0054] Place the sample prepared in step 1 in the center of the sputtering table of the magnetron sputtering equipment. The distance between the target and the substrate is constant at 5 cm, and the sputtering table speed is set to 3 rpm. A Ti target with a purity of 99.99% is selected. Before deposition, the target is sputtered and cleaned in a pure argon environment of 10 Pa for 10 minutes. Then oxygen and argon are introduced in a ratio of 2:10. The sputtering power is set to 100w, and the sputtering time is 60min. After the sputtering is completed, continue to keep it in the vacuum chamber for 20 minutes. The TiO2 coating sample is obtained (recorded as T-1).

[0055] Comparative Example 3

[0056] The same as Example 1, except that the treatment of step 4 is not performed.

[0057] The specific steps are as follows:

[0058] The sample prepared in step 1 is placed in the center of the sputtering table of the magnetron sputtering equipment, the distance between the target and the substrate is constant at 5cm, and the sputtering table speed is set to 3rpm. A Ti target with a purity of 99.99% is selected. Before deposition, the target is sputtered and cleaned in a pure argon environment of 10Pa for 10min. Then oxygen and argon are introduced at a ratio of 2.:10. The sputtering power is set to 100w, and the sputtering time is 60min. After sputtering, it is continued to be stored in the vacuum chamber for 20min. Then the sample is placed in the center of the sputtering table of the magnetron sputtering equipment, the distance between the target and the substrate is constant at 5cm, and the sputtering table speed is set to 3rpm. A Ag target with a purity of 99.99% is selected. Before deposition, the target is sputtered and cleaned in a pure argon environment of 10Pa for 10min. Then argon is introduced at a rate of 20ml / min. The sputtering power is set to 70w, and the sputtering time is 10min. After sputtering, it is continued to be stored in the vacuum chamber for 20min. The TiO2 / Ag coating sample was obtained (denoted as TA-1).

[0059] The following mechanical properties, tribological properties, and corrosion resistance performance tests were performed on the Q235 carbon steel sample, TiO2 coating sample, TiO2 / Ag coating sample, and Mefp-1 / TiO2 / Ag coating sample according to the present invention. The mechanical performance indexes are shown in Table 1, the corrosion resistance indexes are shown in Table 2, and the tribological performance indexes are shown in Table 3.

[0060] Table 1: Mechanical properties test results of Example 1

[0061]

[0062]

[0063] Table 2: Tribological performance test results of Example 1

[0064]

[0065] Table 3: Corrosion resistance test results of Example 1

[0066]

[0067] Table 4: Corrosion resistance and tribological properties test results of Example 2

[0068]

[0069] Table 5: Corrosion resistance and tribological properties test results of Example 3

[0070]

[0071] Table 6: Corrosion resistance and tribological properties test results of Example 4

[0072]

[0073] The critical load and elastic modulus of TiO2 coating, TiO2 / Ag coating and Mefp-1 / TiO2 / Ag coating were tested by nanoscratch and nanoindentation methods, and the adhesion energy of each coating was calculated. The scratch test was carried out with a spherical diamond stylus. The scratch length was 800um, the load increased uniformly from 3mN to 60mN, and the loading time was 60s. The friction force between the slider and the coating during the sliding process changes as shown in the figure. Figure 1As shown. It is generally believed that the mutation point of friction force is the failure point of the coating, and the corresponding loading pressure at this point is the critical load of the coating. The critical loads of TiO2 coating and TiO2 / Ag coating are 24.27mN and 36.45mN, respectively; and the critical load of Mefp-1 / TiO2 / Ag coating prepared by the present invention is 50.35mN, which shows that the composite coating has a stronger ability to bear loads. A Berkovich indenter was used for nanoindentation experiment to test the elastic modulus of the coating. The thickness of the coating was tested using a topography profiler. Combined with the above experimental results, the calculated adhesion energy of the coating is shown in Table 1. The adhesion energy of the TiO2 coating and the TiO2 / Ag coating are 222.54J m -2 and 949.04 J m -2 The adhesion energy of the Mefp-1 / TiO2 / Ag coating prepared by the present invention is 3428.70 J m -2 Its adhesion energy is much higher than that of ordinary magnetron sputtering coatings. Therefore, compared with traditional magnetron sputtering coatings, this coating has better adhesion properties.

[0074] In addition, the friction and wear properties of the substrate and each coating sample were characterized by using a UMT-3 linear reciprocating friction machine. The friction pair used a small Si3N4 steel ball with a diameter of 4 mm, and the grinding material was a Q235 carbon steel substrate and each film layer sample. The specific experimental parameters were set as follows: reciprocating frequency 2 Hz, sliding stroke 6 mm, loading load 1 N, and the corresponding maximum Hertzian contact stress was 0.6 GPa. The experimental time was 30 min. The values ​​of the friction coefficient and wear scar width of each sample are shown in Tables 2, 4, 5 and 6. The wear scar width of Q235 carbon steel is 546 μm, the steady-state friction coefficient is 0.969, and the wear loss is 8.375×10 -5 mm 3 Nm -1 The wear scar width of the Mefp-1 / TiO2 / Ag composite coating prepared by the present invention is only 175 μm, and the steady-state friction coefficient is 0.236. The wear rate is 1.826×10 - 5 mm 3 Nm -1 It is only 21.8% of the base sample. It can be seen that the tribological properties of the coating are significantly improved.

[0075] Regarding the corrosion resistance of the coating, electrochemical experiments were used to characterize the corrosion performance of the Q235 substrate, TiO2 coating sample, TiO2 / Ag coating sample and Mefp-1 / TiO2 / Ag coating sample. The above samples were used as working electrodes, saturated Ag / AgCl electrode and platinum mesh electrode were used as reference electrode and counter electrode respectively, to form a three-electrode system for measuring its alternating current impedance spectrum (EIS). The sample was immersed in a 1wt.% NaCl solution, and an EIS test was performed every 24 hours. The Ro(RpQ) circuit was used for fitting, in which the polarization resistance (Rp) reflects the corrosion resistance of the sample. The experimental results are shown in Tables 3-6 and Figure 3 As shown. The polarization resistance value of carbon steel has remained at 1.3kΩcm -2 The polarization resistance value of the Mefp-1 / TiO2 / Ag composite coating prepared by the present invention increases with the increase of immersion time. After 48 hours, the Rp value increases to 2.742 kΩcm -2 After 120 hours of immersion, the Rp value increased to 3.889 kΩcm -2 It can be seen that the composite coating has an obvious anti-corrosion effect on carbon steel, and the anti-corrosion effect becomes more obvious with the increase of immersion time.

[0076] By adjusting the process (increasing the magnetron sputtering time in step 2 and step 3 or changing the spin coating speed), the thickness of the composite coating prepared according to the implementation process of Example 2 is 6747.3nm, which is increased compared with the Mefp-1 / TiO2 / Ag composite coating prepared in Example 1. The corrosion resistance and friction and wear test results of the composite coating are shown in Table 4. After immersion for 48h and 120h, the Rp values ​​of Example 2 are 2.751kΩcm 2 、3.904kΩcm 2 , which are much higher than those of the substrate sample. It can be seen that the composite coating with adjusted film thickness still has excellent corrosion resistance. In addition, the stable friction coefficient of the Mefp-1 / TiO2 / Ag composite coating is 0.228, the wear scar width is 186um, and the wear rate is 1.944×10 -5 mm 3 Nm -1 .It can be seen that the tribological properties are also significantly improved compared with the Q235 carbon steel sample. In addition, as the magnetron sputtering time increases, the thickness of the Mefp-1 / TiO2 / Ag coating increases. However, when the magnetron sputtering time is further extended, the thickness increase is not obvious, and the density of the coating will decrease. Its corrosion resistance and wear resistance will also decrease. And the energy consumption in the preparation process will increase.

[0077] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0078] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a composite coating material containing mussel byssus protein, characterized in that Here are the steps: S1. Clean the surface of carbon steel and remove the surface oxide film; S2. Preparation of TiO2 layer on carbon steel surface by DC magnetron sputtering; S3. Prepare Ag layer on carbon steel surface by DC magnetron sputtering; S4. Using the TiO2 / Ag film on the carbon steel surface as the precursor film, a layer of Mef -1 protein solution, obtained for carbon steel surface Mef -1 / TiO2 / Ag composite coating; The step S2 specifically comprises selecting a Ti target material with a purity of 99.99%, placing the treated carbon steel at the center of the sputtering table of the magnetron sputtering equipment, keeping a constant distance between the target material and the substrate, introducing argon and oxygen, and the magnetron sputtering power is 80-120w, and the magnetron sputtering time is 40-80min; The step S3 specifically comprises selecting an Ag target material with a purity of 99.99%. Before deposition, the target material is sputtered and cleaned in a pure argon environment of 10 Pa for 10 minutes, and argon gas is introduced at a rate of 10 to 30 ml / min, the magnetron sputtering power is 50 to 90 w, and the magnetron sputtering time is 5 to 30 minutes; The step S1 specifically comprises the following steps: grinding the surface of the carbon steel substrate with water sandpaper, and then polishing it with diamond polishing paste and real velvet polishing cloth, the roughness of which is less than 0.3 μm after polishing, and removing the oxide film on the surface; then rinsing the carbon steel substrate with deionized water, and then putting it into anhydrous ethanol for ultrasonic cleaning, and then taking it out and rinsing it with deionized water and drying it for later use; In step S4 Mef -1 protein solution Mef -1 protein-based solution, diluted with citric acid solution, pH 5-9, concentration 0.05-0.2 mg / mL; In step S4, the glue homogenizer first performs low-speed spin coating and then high-speed spin coating, the low-speed spin coating speed is 500-1000rpm, the low-speed spin coating time is 10-30s, the high-speed spin coating speed is 2000-4000rpm, and the high-speed spin coating time is 50-70s.

2. The method for preparing a composite coating material containing mussel byssin according to claim 1, characterized in that: The target material was sputtered and cleaned in a pure argon environment of 10 Pa for 10 minutes before deposition, with a constant distance of 5 cm and a sputtering table speed set to 3 rpm. After the sputtering was completed, it was kept in the vacuum chamber for 20 minutes.

3. A composite coating material containing mussel byssus protein, characterized in that: The composite coating material is prepared by the preparation method of a composite coating material containing mussel byssin as claimed in claim 1 or 2.

Citation Information

Patent Citations

  • Method for forming amorphous tantalum coating on carbon steel surface through magnetron sputtering deposition

    CN109468601A

  • The manufacturing process of antibacterial, self-cleaning, and wear-resistant hybrid coatings on glazed ceramic substrates

    CA3128998A1

  • Method to obtain a corrosion-resistant and shiny substrate

    CN101370961A

  • Preparation method of gradient abrasion-resistant coating containing Ag nano-particles

    CN107779814A

  • Stainless steel-based fuel cell bipolar plate surface composite coating and preparation method thereof

    CN112609165A