Thin-wall ear ring structure and preparation method thereof and hydraulic device of aircraft constant speed transmission system

By arranging a laser additive layer on the surface of the ear loop base body and forming a wear layer, the problem of ear loop structural wear is solved, the hardness and wear resistance are improved, the service life is extended and the production cost is reduced, and the problem of mechanical hydraulic constant speed transmission is solved. The problem of difficult processing of the ear loop structure in the device.

CN117780587BActive Publication Date: 2024-10-22GUANGDONG INST OF NEW MATERIALS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311755200.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-19
Publication Date
2024-10-22
Estimated Expiration
2043-12-19

AI Technical Summary

Technical Problem

The ear loop structure in the mechanical hydraulic constant speed transmission device has a long manufacturing cycle and high cost due to its small size and precision structure, which affects the promotion and application of the device.

Method used

Using a thin-walled ear loop structure, a laser additive layer is set on the surface of the ear loop base body, and a remelted wear layer is formed on the surface. The wear layer has a directionally arranged microcrystalline structure, which improves the friction and wear properties of the material and controls Wear and protect vital structures.

Benefits of technology

The high hardness and wear resistance of the ear loop structure is achieved, extending the service life, reducing production costs and manufacturing cycles, and improving the stability of the hydraulic device of the aircraft's constant speed transmission system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117780587B_ABST
    Figure CN117780587B_ABST
Patent Text Reader

Abstract

This invention discloses a thin-walled lug structure, its preparation method, and a hydraulic device for an aircraft constant-speed transmission system, belonging to the field of surface protection technology. The thin-walled lug structure includes a lug substrate and a laser additive layer disposed on the surface of the lug substrate. The surface area of ​​the laser additive layer has a wear layer formed after remelting; the wear layer has a directionally aligned microcrystalline structure. This thin-walled lug structure has good hardness and wear resistance. The wear layer can replace the wear effect of the substrate. When the substrate or wear layer of the lug component is partially or completely damaged, the entire wear layer can be used for rapid restoration, effectively protecting the surface of the component. Its preparation method is efficient, low-cost, and easy to operate. The hydraulic device for an aircraft constant-speed transmission system with the above-mentioned thin-walled lug structure has a long service life and high stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surface protection, and in particular to a thin-wall ear ring structure and a preparation method thereof, and a hydraulic device of an aircraft constant speed transmission system. Background Art

[0002] The aircraft constant speed transmission is a special device that transmits the power of the aircraft engine to the aircraft AC generator and converts the variable input speed of the engine into a constant output speed. Among them, the mechanical hydraulic constant speed transmission is a type of constant speed device, which has the advantages of reliable operation, high efficiency (up to 85%), and small size, and is widely used.

[0003] The mechanical hydraulic constant speed transmission device is composed of differential planetary gears, hydraulic pumps, hydraulic motors, speed reducers, protectors and oil circuit systems. The input shaft of the differential planetary gear is connected to the output shaft of the engine, the compensation gear is connected to the hydraulic motor, and the output shaft is connected to the generator. When the speed of the aircraft engine changes or the load changes, causing the generator speed to deviate from the rated value, the speed control system will be activated, appropriately changing the inclination angle of the movable swash plate in the hydraulic pump, changing the pump oil volume to change the motor speed, and thus restoring the generator speed to the rated value. In this constant speed transmission device, both the gear system and the pump-motor transmit power, and the transmission of the gear system is more dominant, so the reliability of the gear system determines the safety and reliability of the constant transmission system.

[0004] In mechanical constant pressure constant speed transmission devices, the ear ring structure is the most representative component structure, such as Figure 1 and Figure 2 As shown, it has a typical hollow structure and a boss on the surface (about 0.2mm). The hollow part is used to assemble the roller of the bearing, and the tiny boss structure on the surface plays a role of fitting and pressing. It is used as a worn part in the matching friction of the pump swash plate ear ring to protect more important parts. However, due to the small geometric size of the ear ring, the precise structure, and frequent wear and tear, the ear ring structure has a long processing and manufacturing cycle and high cost, which seriously affects the promotion and application of the mechanical constant pressure constant speed transmission system in the actual production process.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The object of the present invention is to provide a thin-wall ear ring structure and a preparation method thereof and a hydraulic device of an aircraft constant speed transmission system to solve or improve the above technical problems.

[0007] This application can be implemented as follows:

[0008] In a first aspect, the present application provides a thin-walled ear ring structure, which includes an ear ring base and a laser additive layer arranged on the surface of the ear ring base, wherein the surface area of ​​the laser additive layer has a wear layer formed after remelting; the wear layer has a directionally arranged microcrystalline structure.

[0009] In an optional embodiment, the thickness of the laser additive layer is 100-500 μm, and / or the thickness of the wear layer is 50-250 μm.

[0010] In an optional embodiment, the material of the ear loop substrate is high-strength metal and its alloy; and / or the material of the laser additive layer is Fe-based material.

[0011] In an optional embodiment, the ear loop base is made of low-carbon alloy structural steel.

[0012] In an optional embodiment, the hardness of the material of the laser additive layer is in the range of HRC 42-50.

[0013] In an optional embodiment, the Fe-based material contains 0.1-0.2 wt% C, 2-4 wt% B and Si, 14-18 wt% Cr, 2-3 wt% Mo and 2-5 wt% Ni, and the balance is Fe and inevitable impurities.

[0014] In a second aspect, the present application provides a method for preparing a thin-walled ear ring structure as described in any of the aforementioned embodiments, comprising the following steps: preparing a laser additive layer on the surface of the ear ring substrate, and remelting the surface area of ​​the laser additive layer to form a wear layer.

[0015] In an optional embodiment, the additive manufacturing method of the laser additive layer includes powder feeding additive manufacturing or powder spreading additive manufacturing.

[0016] In an optional embodiment, the laser used in the laser additive layer preparation process includes a solid laser or a gas laser; preferably, a solid laser is used.

[0017] In an optional embodiment, the solid-state laser comprises a pulsed laser beam laser or a continuous laser beam laser; preferably, a pulsed laser beam laser is used.

[0018] In an optional embodiment, the preparation conditions of the laser additive layer include: the average laser power is 500W-2000W, the laser defocus is -20mm to +20mm, the spot size is 1mm-5mm, the scanning speed is 100mm / min-500mm / min, and the overlap rate is 30%-70%.

[0019] In an optional embodiment, the preparation of the wear layer includes: performing secondary laser processing on the surface area of ​​the laser additive layer.

[0020] In an optional embodiment, the laser used in the process of preparing the wear layer is a pulsed laser beam laser.

[0021] In an optional embodiment, the preparation conditions of the wear layer include: laser power of 500W-1000W, laser defocus of 0mm to 20mm, spot size of 2mm-6mm, scanning speed of 100mm / min-600mm / min, and overlap rate of 20%-80%.

[0022] In an optional embodiment, before preparing the laser additive layer, the ear loop substrate is also pre-treated.

[0023] In an optional embodiment, the pretreatment includes degreasing, roughening and preheating and drying the ear loop substrate in sequence.

[0024] In a third aspect, the present application provides a hydraulic device of an aircraft constant speed transmission system, which includes the thin-walled ear ring structure of any one of the aforementioned embodiments.

[0025] The beneficial effects of this application include:

[0026] This application sets a laser additive layer on the surface of the ear ring substrate, and obtains a metallurgical structure that is closely integrated with the thin wall structure in the laser additive method. In addition, the laser additive layer has the characteristics of dense structure and no defects such as holes and cracks. On this basis, a wear layer is formed on the surface area of ​​the laser additive layer through secondary laser treatment. The wear layer has a directional microcrystalline structure that can significantly change the friction and wear properties of the material, play a role in controlling wear and tear and protecting important structures.

[0027] The thin-walled ear ring structure has good hardness and wear resistance, wherein the wear layer can replace the wear effect of the base. When the base or the wear layer of the ear ring component is partially or completely damaged, the wear layer can be used for rapid recovery, which plays a good role in protecting the surface of the component. The preparation method is efficient, low-cost and easy to operate. The hydraulic device of the aircraft constant speed transmission system with the above-mentioned thin-walled ear ring structure has a long service life and high stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0029] Figure 1 This is a schematic structural diagram of the thin-wall ear ring structure of the present application at a first viewing angle;

[0030] Figure 2 This is a schematic structural diagram of the thin-wall ear ring structure of the present application at a second viewing angle;

[0031] Figure 3 This is a microstructure image of a cross section of an additive coating provided in Example 1 of the present application;

[0032] Figure 4 This is a cross-sectional microstructure image of the wear layer and the unremelted laser additive layer after S3 treatment in Example 1 of the present application;

[0033] Figure 5 This is a microstructure image of a cross section of an additive coating provided in Example 2 of the present application;

[0034] Figure 6 This is a cross-sectional microstructure image of the wear layer and the unremelted laser additive layer after S3 treatment in Example 2 of the present application;

[0035] Figure 7 This is a microstructure image of a cross section of an additive coating provided in Example 3 of the present application;

[0036] Figure 8 This is a cross-sectional microstructure diagram of the wear layer and the unremelted laser additive layer after S3 treatment in Example 3 of the present application. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0038] The thin-wall ear ring structure and its preparation method and the hydraulic device of the aircraft constant speed transmission system provided by the present application are specifically described below.

[0039] The present application proposes a thin-walled ear ring structure, which includes an ear ring substrate and a laser additive layer arranged on the surface of the ear ring substrate, wherein the surface area of ​​the laser additive layer has a wear layer formed after remelting; the wear layer has a directionally arranged microcrystalline structure.

[0040] In other words, the laser additive layer (positioned as the initial laser additive layer) arranged on the surface of the ear ring base ultimately includes an unremelted portion and a remelted portion, wherein the unmelted portion still serves as a laser additive layer (defined as the final laser additive layer), and the remelted portion serves as a wear layer.

[0041] This application sets a laser additive layer on the surface of the ear ring substrate, and obtains a metallurgical structure that is closely integrated with the thin wall structure in the laser additive method. In addition, the laser additive layer has the characteristics of dense structure and no defects such as holes and cracks. On this basis, a wear layer is formed on the surface area of ​​the laser additive layer through secondary laser treatment. The wear layer has a directional microcrystalline structure that can significantly change the friction and wear properties of the material, play a role in controlling wear and tear and protecting important structures.

[0042] For reference, the thickness of the laser additive layer can be 100-500μm, such as 100μm, 150μm, 200μm, 250μm, 300μm, 350μm, 400μm, 450μm or 500μm, etc., or any other value within the range of 100-500μm. It is worth noting that the thickness of the "laser additive layer" here is the total thickness of the substrate surface coating (the thickness of the initial laser additive layer), that is, the sum of the thickness of the unremelted additive layer and the thickness of the wear layer formed after remelting, which can also be understood as: the thickness of the initial laser additive layer = the thickness of the final additive layer + the thickness of the wear layer.

[0043] The thickness of the wear layer may be 50-250 μm, such as 50 μm, 80 μm, 100 μm, 120 μm, 150 μm, 180 μm, 200 μm, 220 μm or 250 μm, or any other value within the range of 50-250 μm.

[0044] In the present application, the material of the ear ring base is high-strength metal and its alloy, which has the characteristics of high strength and dimensional stability. For example, the material of the ear ring base can be low-carbon alloy structural steel, which has high strength, good comprehensive performance and processing performance, and can be treated with different heat treatment processes and surface treatment processes to make the local surface have special properties.

[0045] The material of the laser additive layer is Fe-based material. For reference, the hardness range of the material of the laser additive layer can be HRC 42-50. If the HRC hardness of the material of the laser additive layer is lower than 42, the wear time will not meet the requirements; if the HRC hardness of the material of the laser additive layer is higher than 50, the wear on the wear part will increase.

[0046] In some embodiments, the Fe-based material used for the laser additive layer may contain 0.1-0.2wt% (such as 0.1wt%, 0.15wt% or 0.2wt%) of C, 2-4wt% (such as 2wt%, 2.5wt%, 3wt%, 3.5wt% or 4wt%) of B and Si (i.e., the total amount of B and Si is 2-4wt%), 14-18wt% (such as 14wt%, 15wt%, 16wt%, 17wt% or 18wt%) of Cr, 2-3wt% (such as 2wt%, 2.5wt% or 3wt%) of Mo, and 2-5wt% (such as 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% or 5wt%) of Ni, and the remainder is Fe and unavoidable impurities. The Fe-based material containing the above-mentioned element composition has similar temperature stability, structural rigidity and plastic elastic deformation properties as the matrix material. Moreover, its thermal expansion coefficient is relatively close to that of the low-carbon alloy structural steel.

[0047] As mentioned above, the thin-walled ear ring structure provided by the present application has good hardness and wear resistance, the laser additive layer and the substrate have good metallurgical bonding, and the wear layer can replace the wear effect of the substrate without affecting the organizational structure and performance of the substrate. When the substrate or wear layer of the ear ring component is partially or completely damaged, the wear layer can be used for rapid recovery, which plays a good role in protecting the surface of the component.

[0048] Correspondingly, the present application also provides a method for preparing the above-mentioned thin-walled ear ring structure, which may include the following steps: preparing a laser additive layer on the surface of the ear ring substrate, and remelting the surface area of ​​the laser additive layer to form a wear layer.

[0049] Before preparing the laser additive layer, the ear loop substrate may be pre-treated.

[0050] For reference, the pretreatment may include degreasing, roughening and preheating and drying the ear loop substrate in sequence.

[0051] Specifically, after the substrate is degreased and deoiled, the non-laser processed parts can be protected with fixtures or masking tape. The oxide layer on the surface of the substrate is removed by grinding to increase the surface activity and improve the bonding between the cladding layer and the substrate. Furthermore, the substrate is preheated in an electric furnace to reduce the water content in the surface layer of the substrate, reduce the thermal expansion stress of the substrate and the laser additive layer, and reduce deformation. It should be noted that the above-mentioned degreasing, grinding and preheating and drying steps are all common technologies in this field, and the specific processing parameters are not limited too much here.

[0052] Alternatively, the additive manufacturing method of the laser additive layer in the present application may include, for example, powder feeding additive manufacturing or powder spreading additive manufacturing. The powder or wire material is fed into a molten pool formed by the laser and heated to a molten state, and melted together with a portion of the matrix material to form a molten pool, and then the molten pool solidifies under the heat conduction of the matrix material to form a metallurgical bond with each other.

[0053] In some preferred embodiments, a powder feeding additive manufacturing method is used to prepare the laser additive layer. This method is extremely flexible, the laser beam has sufficient energy to control the melting of the coating material, the cladding process does not cause substantial damage to the substrate, the laser parameters are easy to control, the thickness of the cladding layer is controllable, and the obtained laser additive layer has high bonding strength with the substrate and good stability. In addition, this method also has the advantages of high efficiency and low cost.

[0054] For reference, the laser used in the above-mentioned laser additive layer preparation process may include, for example, a solid laser or a gas laser, preferably a solid laser. Both gas lasers and solid lasers can achieve additive manufacturing, but gas lasers produce laser beams with a wavelength of 10.6 microns, and solid lasers produce laser beams with a wavelength of 1.06 microns. The absorption rate of metals to laser beams of the two wavelengths is very different. To achieve the same cladding effect, the total energy input of solid lasers is much lower than that of gas lasers, and the thermal impact and thermal deformation on the substrate are much lower, so solid lasers are preferred.

[0055] Among them, the solid laser can be a pulsed laser beam laser or a continuous laser beam laser; preferably, a pulsed laser beam laser is used. The heat input of a continuous laser beam laser is continuous, and the formed laser molten pool is always in a high temperature state, while the heat input of a pulsed laser beam laser is intermittent, which has a significant cooling effect on the formed laser molten pool. The average temperature of the molten pool is significantly lower than that of a continuous laser, so the thermal impact on the substrate is significantly smaller, so a pulsed laser beam laser is preferred.

[0056] Exemplarily, the preparation conditions of the laser additive layer in the present application may include: the average laser power is 500W-2000W (such as 500W, 800W, 1000W, 1200W, 1500W, 1800W or 2000W, etc.), the laser defocus is -20mm to +20mm (such as -20mm, -15mm, -10mm, -5mm, 0mm, +5mm, +10mm, +15mm or +20mm, etc.), the spot size is 1mm-5mm (such as 1mm, 1.5mm, 2mm, 2.5mm, 3mm , 3.5mm, 4mm, 4.5mm or 5mm, etc.), the scanning speed is 100mm / min-500mm / min (such as 100mm / min, 150mm / min, 200mm / min, 250mm / min, 300mm / min, 350mm / min, 400mm / min, 450mm / min or 500mm / min, etc.), the overlap rate is 30%-70% (such as 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65% or 70%, etc.).

[0057] If the average laser power is less than 500W, it is not conducive to the formation of a continuous cladding layer; if the laser power is greater than 2000W, it is easy to cause powder spheroidization, severe spatter, poor surface forming of the cladding layer, and an increase in the range of the heat-affected zone. If the laser defocus exceeds 20mm, it is not conducive to the effective convergence of the laser beam and the coordination with the powder. If the spot size is less than 1mm, it is easy to cause excessive melting of the matrix and powder and too low additive efficiency; if the spot size is greater than 5mm, it is easy to cause the laser beam energy density to be too low or unable to do fine additive in a small range. If the scanning speed is less than 100mm / min, it is easy to cause overheating of the matrix and cause serious deformation; if the scanning speed is greater than 500mm / min, it is easy to cause a large range of poor bonding areas in the initial section of additive manufacturing. If the overlap rate is less than 30%, it is easy to increase the surface roughness of the cladding layer of additive manufacturing, thereby generating more interlayer defects when multi-layer additive manufacturing is performed; if the overlap rate is greater than 70%, it is easy to increase the single-layer thickness of the cladding layer of additive manufacturing, thereby generating more intra-layer defects when multi-pass additive manufacturing is performed.

[0058] In the present application, the preparation of the wear layer includes: performing laser secondary processing on the surface area of ​​the laser additive layer.

[0059] The laser used in the preparation process is preferably a pulsed laser beam laser.

[0060] In some preferred embodiments, the equipment and method used to prepare the laser additive layer and the wear layer are consistent, and both use a pulsed laser beam laser.

[0061] Exemplarily, the preparation conditions of the wear layer in the present application may include: a laser power of 500W-1000W (such as 500W, 600W, 700W, 800W, 900W or 1000W, etc.), a laser defocus of 0mm to 20mm (such as 0mm, 5mm, 10mm, 15mm or 20mm, etc.), a spot size of 2mm-6mm (such as 2mm, 3mm, 4mm, 5mm or 6mm, etc.), a scanning speed of 100mm / min-600mm / min (such as 100mm / min, 200mm / min, 300mm / min, 400mm / min, 500mm / min or 600mm / min, etc.), and an overlap rate of 20%-80% (such as 20%, 30%, 40%, 50%, 60%, 70% or 80%, etc.).

[0062] If the average laser power is less than 500W, it is not conducive to the formation of a continuous remelting layer; if the laser power is greater than 1000W, it is easy to cause the surface quality of the remelting layer to deteriorate and the remelting area to be too large. If the laser defocus exceeds 20mm, it is not conducive to the effective convergence of the laser beam energy. If the spot size is less than 2mm, it is easy to cause the surface quality of the remelting layer to deteriorate and the remelting efficiency to be too low; if the spot size is greater than 6mm, it is easy to cause the depth of the remelting layer to be too thin or it is impossible to do fine remelting in a small range. If the scanning speed is less than 100mm / min, it is easy to cause the remelting layer to overheat, resulting in too deep remelting depth and low efficiency; if the scanning speed is greater than 600mm / min, it is easy to cause insufficient heating and reduced remelting degree, resulting in too shallow remelting depth. If the overlap rate is less than 20%, it is easy to cause insufficient overlap of the remelting layer, and the organization and thickness of the remelting layer are difficult to control; if the overlap rate is greater than 80%, it is easy to increase the overlap of the remelting layer, form multiple remelting dendrite organizations, and increase surface unevenness.

[0063] As mentioned above, the preparation method provided in this application is highly efficient, low-cost and easy to operate.

[0064] In addition, the present application also provides a hydraulic device of an aircraft constant speed transmission system, which includes the above-mentioned thin-wall ear ring structure.

[0065] The hydraulic device of the aircraft constant speed transmission system has a long service life and high stability.

[0066] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0067] Example 1

[0068] This embodiment provides a thin-wall ear ring structure, which includes an ear ring base and a laser additive layer arranged on the surface of the ear ring base, and the surface area of ​​the laser additive layer has a wear layer formed after remelting.

[0069] The ear ring substrate is a 12CrNi4MoA substrate. The laser additive layer is made of a Fe-based material, which contains 0.15wt% C, 3wt% B and Si, 16wt% Cr, 2.5wt% Mo and 3.5wt% Ni, and the remainder is Fe and unavoidable impurities, with a hardness of HRC45.

[0070] The preparation of the thin-wall ear loop structure includes:

[0071] S1: Pre-treatment of the ear loop substrate:

[0072] The ear loop substrate is degreased, roughened and preheated and dried.

[0073] S2: A powder feeding additive manufacturing method is used to prepare a laser additive layer on the surface of the pretreated ear loop substrate.

[0074] The laser used in this step is a pulsed laser beam laser. In this embodiment, a pulsed laser beam laser model XL-1000Y produced by Guangzhou Xingre Laser Technology Co., Ltd. is specifically used.

[0075] The preparation conditions of the laser additive layer are as follows: the average laser power is 2000 W, the laser defocus is +20 mm, the spot size is 5 mm, the scanning speed is 500 mm / min, and the overlap rate is 30%.

[0076] S3: Use the equipment and method of S2 to perform secondary laser treatment on the surface area of ​​the laser additive layer, so that the laser additive layer in this area is remelted to form a wear layer.

[0077] The conditions of the secondary laser treatment are as follows: the average laser power is 1000 W, the laser defocus is 20 mm, the spot size is 6 mm, the scanning speed is 600 mm / min, and the overlap rate is 20%.

[0078] Furthermore, the cross section of the substrate surface coating in the thin-walled ear loop structure prepared in this embodiment was placed under an optical microscope for observation, and the results were as follows: Figure 3 As shown. Figure 3 It can be seen that the coating structure prepared in this embodiment is dense, without defects such as holes and cracks, the average total thickness of the coating (non-remelted laser additive layer part + wear layer) is about 500 μm, and the non-remelted laser additive layer part is well bonded to the substrate surface; the thickness of the wear layer is about 250 μm, and the wear layer is well bonded to the non-remelted laser additive layer part, and the dendrite direction in the wear layer is significantly different from that of the non-remelted laser additive layer part (such as Figure 4 ).

[0079] Example 2

[0080] The difference between this embodiment and embodiment 1 is that:

[0081] In S2, the preparation conditions of the laser additive layer are as follows: the average laser power is 1000 W, the laser defocus is -15 mm, the spot size is 4 mm, the scanning speed is 300 mm / min, and the overlap rate is 50%.

[0082] In S3, the conditions for the secondary laser treatment are as follows: the average laser power is 750 W, the laser defocus is 10 mm, the spot size is 4 mm, the scanning speed is 400 mm / min, and the overlap rate is 50%.

[0083] Furthermore, the cross section of the substrate surface coating in the thin-walled ear loop structure prepared in this embodiment was placed under an optical microscope for observation, and the results were as follows: Figure 5 As shown. Figure 5 It can be seen that the coating structure prepared in this embodiment is dense, without defects such as holes and cracks, the average total thickness of the coating (non-remelted laser additive layer part + wear layer) is about 300 μm, and the non-remelted laser additive layer part is well bonded to the substrate surface; the thickness of the wear layer is about 150 μm, and the wear layer is well bonded to the non-remelted laser additive layer part, and the dendrite direction in the wear layer is significantly different from that of the non-remelted laser additive layer part (such as Figure 6 ).

[0084] Example 3

[0085] The difference between this embodiment and embodiment 1 is that:

[0086] In S2, the preparation conditions of the laser additive layer are as follows: the average laser power is 500 W, the laser defocus is +5 mm, the spot size is 1.5 mm, the scanning speed is 100 mm / min, and the overlap rate is 70%.

[0087] In S3, the conditions for the secondary laser treatment are as follows: the average laser power is 550 W, the laser defocus is 8 mm, the spot size is 2 mm, the scanning speed is 100 mm / min, and the overlap rate is 80%.

[0088] Furthermore, the cross section of the substrate surface coating in the thin-walled ear loop structure prepared in this embodiment was placed under an optical microscope for observation, and the results were as follows: Figure 7 As shown. Figure 7 It can be seen that the coating structure prepared in this embodiment is dense, without defects such as holes and cracks, the average total thickness of the coating (non-remelted laser additive layer part + wear layer) is about 100 μm, and the non-remelted laser additive layer part is well bonded to the substrate surface; the thickness of the wear layer is about 50 μm, and the wear layer is well bonded to the non-remelted laser additive layer part, and the dendrite direction in the wear layer is significantly different from that of the non-remelted laser additive layer part (such as Figure 8 ).

[0089] Comparative Example 1

[0090] The difference between this comparative example and Example 1 is that the material of the laser additive layer is Fe-based material, which contains 0.25wt% C, 5wt% B and Si, 19wt% Cr and 1.5wt% Ni, and the remainder is Fe and unavoidable impurities, and its hardness is HRC55.

[0091] Comparative Example 2

[0092] The difference between this comparative example and Example 1 is that step S3 is not performed.

[0093] Comparative Example 3

[0094] The difference between this comparative example and Example 1 is that in S2, the average laser power is 300W.

[0095] Comparative Example 4

[0096] The difference between this comparative example and Example 1 is that in S2, the average laser power is 2500W.

[0097] Comparative Example 5

[0098] The difference between this comparative example and Example 1 is that in S2, the laser defocus amount is +30 mm.

[0099] Comparative Example 6

[0100] The difference between this comparative example and Example 1 is that in S2, the spot size is 0.5 mm.

[0101] Comparative Example 7

[0102] The difference between this comparative example and Example 1 is that in S2, the spot size is 8 mm.

[0103] Comparative Example 8

[0104] The difference between this comparative example and Example 1 is that in S2, the scanning speed is 80 mm / min.

[0105] Comparative Example 9

[0106] The difference between this comparative example and Example 1 is that in S2, the scanning speed is 600 mm / min.

[0107] Comparative Example 10

[0108] The difference between this comparative example and Example 1 is that in S2, the overlap rate is 20%.

[0109] Comparative Example 11

[0110] The difference between this comparative example and Example 1 is that in S2, the overlap rate is 80%.

[0111] Test example

[0112] The thin-walled ear ring structures obtained in Examples 1-3 and Comparative Examples 1-11 were subjected to performance tests, wherein the hardness was measured with reference to GB / T230.1-2018 and the wear resistance was measured with reference to GB / T12444.2-1990. The test results are shown in Table 1.

[0113] Table 1 Test results

[0114]

[0115]

[0116] It can be seen from Table 1 that the thin-walled ear ring structure provided in the embodiment of the present application has a relatively matched hardness and a relatively high wear resistance. It should be noted that, for the thin-walled ear ring structure of the present application, the higher the hardness, the better, but it needs to match the wear resistance, otherwise too high hardness will cause serious wear of the mating parts.

[0117] In summary, the solution provided in this application has at least the following characteristics:

[0118] (1) The coating made on the surface of the thin-walled ear ring structure substrate has good bonding with the substrate and moderate hardness, which can replace the wear effect of the substrate; the coating and the substrate are metallurgically bonded without the risk of falling off, and the production and processing of the coating does not affect the organizational structure and performance of the substrate;

[0119] (2) The laser additive layer formed by laser additive manufacturing can also be directly manufactured multiple times, and the part of the laser additive layer that has not been remelted can also form a good bond with the wear layer. The multiple preparation, processing and service of the wear layer will not affect the thin-wall structure of the ear ring; and when the base or wear layer of the ear ring component is partially or completely damaged, the wear layer can be used entirely for rapid recovery.

[0120] (3) The laser additive manufacturing method used to prepare the wear layer has the characteristics of high efficiency, low cost, and easy operation. There is no need to process the coating surface before remelting. The process is simple and easy to automate.

[0121] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A thin-wall ear ring structure, characterized in that: It comprises an ear loop base and a laser additive layer arranged on the surface of the ear loop base, wherein the surface area of ​​the laser additive layer has a wear layer formed after remelting; and the wear layer has a directional microcrystalline structure; The material of the laser additive layer is Fe-based material; the Fe-based material contains 0.1-0.2wt% C, 2-4wt% B and Si, 14-18wt% Cr, 2-3wt% Mo and 2-5wt% Ni, and the balance is Fe and unavoidable impurities; The preparation of the thin-walled ear ring structure comprises the following steps: preparing the laser additive layer on the surface of the ear ring substrate, and remelting the surface area of ​​the laser additive layer to form the wear layer; the preparation of the wear layer comprises: performing laser secondary treatment on the surface area of ​​the laser additive layer; The preparation conditions of the laser additive layer include: laser average power of 500W-2000W, laser defocus of -20mm to +20mm, spot size of 1mm-5mm, scanning speed of 100mm / min-500mm / min, and overlap rate of 30%-70%; The preparation conditions of the wear layer include: laser power of 500W-1000W, laser defocus of 0mm to 20mm, spot size of 2mm-6mm, scanning speed of 100mm / min-600mm / min, and overlap rate of 20%-80%.

2. The thin-wall ear loop structure according to claim 1, characterized in that: The thickness of the laser additive layer is 100-500 μm, and / or the thickness of the wear layer is 50-250 μm.

3. The thin-wall ear loop structure according to claim 1 or 2, characterized in that: The material of the ear ring base is high-strength metal and its alloy.

4. The thin-wall ear loop structure according to claim 3, characterized in that: The material of the ear ring substrate is low-carbon alloy structural steel.

5. The thin-wall ear loop structure according to claim 1, characterized in that: The hardness of the material of the laser additive layer is in the range of HRC 42-50.

6. A method for preparing the thin-walled ear loop structure according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: preparing the laser additive layer on the surface of the ear loop substrate, and remelting the surface area of ​​the laser additive layer to form the wear layer; The preparation conditions of the laser additive layer include: laser average power of 500W-2000W, laser defocus of -20mm to +20mm, spot size of 1mm-5mm, scanning speed of 100mm / min-500mm / min, and overlap rate of 30%-70%; The preparation of the wear layer comprises: performing a laser secondary treatment on the surface area of ​​the laser additive layer; The preparation conditions of the wear layer include: laser power of 500W-1000W, laser defocus of 0mm to 20mm, spot size of 2mm-6mm, scanning speed of 100mm / min-600mm / min, and overlap rate of 20%-80%.

7. The preparation method according to claim 6, characterized in that: The additive manufacturing method of the laser additive layer includes powder feeding type additive manufacturing or powder spreading type additive manufacturing.

8. The preparation method according to claim 7, characterized in that: The laser used in the laser additive layer preparation process includes a solid laser or a gas laser.

9. The preparation method according to claim 8, characterized in that: The laser used in the laser additive layer preparation process is a solid laser.

10. The preparation method according to claim 9, characterized in that: The solid laser used in the laser additive layer preparation process includes a pulsed laser beam laser or a continuous laser beam laser.

11. The preparation method according to claim 10, characterized in that: The solid laser used in the laser additive layer preparation process is a pulsed laser beam laser.

12. The preparation method according to claim 6, characterized in that: The laser used in the process of preparing the wear layer is a pulsed laser beam laser.

13. The preparation method according to claim 6, characterized in that: Before preparing the laser additive layer, the ear loop substrate is also pre-treated.

14. The preparation method according to claim 13, characterized in that: The pretreatment includes degreasing, roughening and preheating and drying the ear loop substrate in sequence.

15. A hydraulic device for a constant speed transmission system of an aircraft, characterized in that: The invention comprises the thin-wall ear loop structure as described in any one of claims 1 to 5.