Cement composition and method for producing the same
By adjusting the ratio of MgO/Fe2O3+CL'SO3/SO3 in Portland cement and adding alkanolamine, the mineral composition is optimized to solve the problem of long-term strength control of cement under high MgO conditions and achieve the long-term strength of mortar under high MgO content. Lift and strength stability.
Patent Information
- Application Number
- CN202280064674.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-12-23
- Filing Date
- 2022-12-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-12-08
AI Technical Summary
The existing technology is difficult to stably control the long-term strength of cement under high MgO conditions, especially when the dolomite content in limestone mines is high, resulting in deviations in concrete quality performance, and reducing the MgO content needs to be less than 1.9% to prevent strength reduction.
By adjusting the MgO/Fe2O3+CL'SO3/SO3 ratio in Portland cement to 0.55~0.95, and adding 0.001~0.025 parts by mass of alkanolamine, such as diethanol isopropanolamine, the minerals calculated by combining Baugh's formula Composition, optimize the contents of C3S, C2S, C3A, and C4AF to improve the long-term strength of the mortar.
The long-term strength of the mortar is achieved under high MgO content. The addition of alkanolamine promotes the solid solution of the ferrite phase, improves the water tightness and strength of the mortar, and avoids expansion cracks caused by excessive MgO content. The high strength of the mortar is maintained.
Smart Images

Figure CN117999249B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a cement composition and a method for preparing the same. Background Art
[0002] Clinker contains small amounts of components such as Mg, Na, and K, and their contents vary depending on the raw materials.
[0003] For example, in Non-Patent Document 1, it is known that cement under high MgO conditions is replaced with Ca, which is the same alkaline earth metal, and it is known that, as a result, the amount of belite is relatively reduced, and thus the long-term strength at 28 days is reduced, as shown in Non-Patent Document 2. In Non-Patent Document 3, it is found that by increasing SO3, it is possible to improve the strength even with high MgO.
[0004] In addition, Patent Document 1 discloses that if the MgO content in the calcined cement clinker exceeds 1.0 mass %, the strength development of the cement over a long period of time is reduced, and therefore the raw materials are prepared in such a way that the MgO content in the calcined silicate cement clinker becomes less than 1.0 mass %.
[0005] Moreover, Patent Document 2 discloses a cement clinker having a 2CaO·SiO2 content of 30 to 60% by mass as calculated by the Baugh formula, characterized in that the MgO content in the cement clinker is greater than 1.2% by mass and less than 1.9% by mass, and the SO3 content is 0.4 to 1.2% by mass.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2009-013023
[0009] Patent Document 2: Japanese Patent Application Publication No. 2018-65750
[0010] Non-patent literature
[0011] Non-patent document 1: Crystal Chemistry of Tricalcium Silicate Solid Solution, in 5th ISCC, Vol. 1, 61-66 (1969)
[0012] Non-patent document 2: Annual Report on Cement Technology, Vol. 22, 62-66 (1968)
[0013] Non-patent literature 3: Cement Science and Concrete Technology, Vol. 70 Summary of the invention
[0014] Technical issues to be solved by the invention
[0015] However, since the cement composition is adjusted to the high MgO condition, it is difficult to control, and the long-term strength cannot be stably maintained in the methods described in non-patent documents 1 to 3. The problem is that a large amount of dolomite is sometimes contained in the mines that produce limestone as a raw material, and the quality performance of concrete, etc. is deviated due to the high MgO content of the manufactured cement. Therefore, as in patent document 1, it is necessary to reduce the MgO content. In patent document 2, it is explained that even if the MgO content in cement is high, the long-term strength manifestation of cement can be prevented from decreasing, but even so, it is necessary to make the upper limit of the MgO content less than 1.9 mass%.
[0016] An object of the present invention is to provide a cement composition having excellent long-term strength of mortar even when the content of MgO in silicate cement is high, and a method for producing a cement composition capable of improving the long-term strength of mortar even when the content of MgO in silicate cement is high.
[0017] Means for solving technical problems
[0018] The present invention provides the following <1> to <10>.
[0019] <1> A cement composition comprising:
[0020] Portland cement satisfying the following (1) and (2); and
[0021] The alkanolamine is contained in an amount of 0.001 to 0.025 parts by mass based on 100 parts by mass of the silicate cement.
[0022] (1)0.55≤MgO / Fe2O3+CL'SO3 / SO3≤0.95
[0023] (2) 0≤ΔC4AF
[0024] In (1), MgO represents the mass (mass %) of MgO in the silicate cement, Fe2O3 represents the mass (mass %) of Fe2O3 in the silicate cement, SO3 represents the SO3 conversion amount (mass %) of the silicate cement, and CL'SO3 represents the SO3 conversion amount (mass %) of the clinker of the silicate cement.
[0025] In (2), ΔC4AF represents the difference between the mass (mass %) of R.C4AF and the mass (mass %) of B.C4AF (R.C4AF-B.C4AF). R.C4AF represents the C4AF value of the Portland cement measured by a powder X-ray diffraction device, and B.C4AF represents 3.04×Fe2O3. Fe2O3 in B.C4AF represents the mass (mass %) of Fe2O3 in the Portland cement.
[0026] <2> The cement composition according to <1>, wherein
[0027] In (1), the MgO / Fe2O3 exceeds 0.35.
[0028] <3> The cement composition according to <1> or <2>, wherein
[0029] The silicate cement is ordinary silicate cement having C3S of 45-75 mass %, C2S of 5-25 mass %, C3A of 7-11 mass %, and C4AF of 7-11 mass % calculated by Bauer's formula.
[0030] <4> The cement composition according to any one of <1> to <3>, wherein
[0031] The content of the alkanolamine is 0.005 to 0.02 parts by mass relative to 100 parts by mass of the silicate cement.
[0032] <5> The cement composition according to any one of <1> to <4>, wherein
[0033] The alkanolamine is at least one selected from the group consisting of diethanolisopropanolamine, triisopropanolamine, ethanoldiisopropanolamine, triethanolamine, N-methyldiethanolamine, and N-n-butyldiethanolamine.
[0034] <6> A method for producing a cement composition, wherein:
[0035] Portland cement and an alkanolamine are mixed, wherein the Portland cement satisfies the following (1) and (2), and the alkanolamine is contained in an amount of 0.001 to 0.025 parts by mass based on 100 parts by mass of the Portland cement.
[0036] (1)0.55≤MgO / Fe2O3+CL'SO3 / SO3≤0.95
[0037] (2) 0≤ΔC4AF
[0038] In (1), MgO represents the mass (mass %) of MgO in the silicate cement, Fe2O3 represents the mass (mass %) of Fe2O3 in the silicate cement, SO3 represents the SO3 conversion amount (mass %) of the silicate cement, and CL'SO3 represents the SO3 conversion amount (mass %) of the clinker of the silicate cement.
[0039] In (2), ΔC4AF represents the difference between the mass (mass %) of R.C4AF and the mass (mass %) of B.C4AF (R.C4AF-B.C4AF). R.C4AF represents the C4AF value of the Portland cement measured by a powder X-ray diffraction device, and B.C4AF represents 3.04×Fe2O3. Fe2O3 in B.C4AF represents the mass (mass %) of Fe2O3 in the Portland cement.
[0040] <7> The method for producing a cement composition according to <6>, wherein
[0041] In (1), the MgO / Fe2O3 exceeds 0.35.
[0042] <8> The method for producing a cement composition according to <6> or <7>, wherein
[0043] The silicate cement is ordinary silicate cement having C3S of 45-75 mass %, C2S of 5-25 mass %, C3A of 7-11 mass %, and C4AF of 7-11 mass % calculated by Bauer's formula.
[0044] <9> The method for producing a cement composition according to any one of <6> to <8>, wherein
[0045] The amount of the alkanolamine added is 0.005 to 0.02 parts by mass relative to 100 parts by mass of the silicate cement.
[0046] <10> The method for producing a cement composition according to any one of <6> to <9>, wherein
[0047] The alkanolamine is at least one selected from the group consisting of diethanolisopropanolamine, triisopropanolamine, ethanoldiisopropanolamine, triethanolamine, N-methyldiethanolamine, and N-n-butyldiethanolamine.
[0048] Effects of the Invention
[0049] According to the present invention, there can be provided a cement composition having excellent long-term strength of mortar even when the MgO content in Portland cement is high, and a method for producing a cement composition capable of improving the long-term strength of mortar even when the MgO content in Portland cement is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 The conditions for the examples and comparative examples are shown in FIG. ** Graph of the ΔC4AF values.
[0051] Figure 2 The conditions for the 7-day and 28-day periods of the examples and comparative examples are plotted. ** Graph of the values of the mortar improvement strength difference. DETAILED DESCRIPTION
[0052] The notation of the numerical range of "AA to BB" in this specification means "AA or more and BB or less".
[0053] <Cement composition>
[0054] The cement composition of the present invention comprises: Portland cement satisfying the following (1) and (2); and 0.001 to 0.025 parts by mass of an alkanolamine based on 100 parts by mass of the Portland cement.
[0055] (1)0.55≤MgO / Fe2O3+CL'SO3 / SO3≤0.95
[0056] (2) 0≤ΔC4AF
[0057] In (1), MgO represents the mass (mass %) of MgO in Portland cement, Fe2O3 represents the mass (mass %) of Fe2O3 in Portland cement, SO3 represents the SO3 equivalent amount (mass %) of Portland cement, and CL'SO3 represents the SO3 equivalent amount (mass %) of Portland cement clinker.
[0058] In (2), ΔC4AF represents the difference between the mass (mass %) of R.C4AF and the mass (mass %) of B.C4AF (R.C4AF-B.C4AF). R.C4AF represents the C4AF value of silicate cement measured by a powder X-ray diffraction device, and B.C4AF represents 3.04×Fe2O3. Fe2O3 in B.C4AF represents the mass (mass %) of Fe2O3 in silicate cement.
[0059] Hereinafter, the silicate cement satisfying the above (1) and (2) will be referred to as "the silicate cement of the present invention" or simply "the cement of the present invention".
[0060] In other words, the cement composition of the present invention comprises clinker, gypsum and alkanolamine, the Portland cement comprising clinker and gypsum satisfies the above (1) and (2), and the content of alkanolamine is within the above range.
[0061] When the MgO content in cement is high, for example, 1.30 mass % or more, the hydration of calcium decreases, so the strength of mortar or the like is relatively reduced.
[0062] It is known to use additives such as alkanolamines to improve strength. However, the strength improvement expected from alkanolamines is only the short-term strength of less than 7 days, and the long-term strength tends to decrease.
[0063] However, by setting the content of the cement composition to the above structure, the long-term strength of the mortar can be improved. The reason is not clear, but it is estimated to be based on the following reasons.
[0064] [Condition (1)]
[0065] Condition (1) is that "MgO / Fe2O3+CL'SO3 / SO3" is 0.55 to 0.95.
[0066] Although the details are not clear, it is believed that the increase in the mass of MgO relative to the mass of Fe2O3, or the increase in the SO3 conversion amount (mass basis) in the clinker relative to the SO3 conversion amount (mass basis) in the cement, is related to the solid solution of the ferrite phase. For example, "MgO / Fe2O3+CL'SO3 / SO3" can be considered as an indicator of the solid solution amount of the ferrite phase.
[0067] It is believed that the alkanolamine contained together with the silicate cement in the present invention has the function of promoting water tightness and increasing the strength of the mortar by dissolving iron and the like in the ferrite phase and making it dissolve in the gel and penetrate uniformly. Therefore, magnesium and SO3 are solid-dissolved in the ferrite phase, and the effect of enhancing the strength of the mortar by the alkanolamine is further improved, which can improve the long-term strength of the mortar.
[0068] When "MgO / Fe2O3+Cl'SO3 / SO3" is less than 0.55, the solid solution amount of the ferrite phase is small, the effect of enhancing the mortar strength by the alkanolamine cannot be fully obtained, and the long-term strength of the mortar is not excellent.
[0069] If "MgO / Fe2O3+Cl'SO3 / SO3" exceeds 0.95, it is difficult to obtain the effect of improving strength by alkanolamine, and excessive amounts of alkanolamine, unreacted MgO and MgSO4 respectively cause expansion cracks and fail to maintain mortar strength.
[0070] From the viewpoint of further improving the long-term strength of the mortar, "MgO / Fe2O3+CL'SO3 / SO3" is preferably 0.60 to 0.90, more preferably 0.70 to 0.80.
[0071] Furthermore, in condition (1), MgO / Fe2O3 is preferably greater than 0.35.
[0072] It is considered that the mass of MgO relative to the mass of Fe2O3 in cement represents the solid solution amount of C4AF, and when MgO / Fe2O3 exceeds 0.35, the solid solution of C4AF can be promoted.
[0073] From the viewpoint of increasing the amount of solid solution of the ferrite phase, MgO / Fe2O3 is preferably 0.36 to 0.60, more preferably 0.40 to 0.50.
[0074] From the viewpoint of increasing the amount of alkanolamine dissolved in solid, the mass of MgO in condition (1), that is, MgO in cement, is preferably 3.5 mass% or less, more preferably 0.5 to 3.0 mass%, and even more preferably 1.0 to 2.5 mass%.
[0075] From the viewpoint of solid solution stabilization of the ferrite phase, the mass of Fe2O3 in condition (1), i.e., Fe2O3 in cement, is preferably 2.0 to 4.0 mass %, more preferably 2.5 to 3.5 mass %, and still more preferably 2.7 to 3.4 mass %.
[0076] From the viewpoint of promoting the solid solution of C4AF and ensuring the fluidity of cement, the CL'SO3 in condition (1), that is, the SO3 conversion amount of clinker is preferably 2.5 mass% or less, more preferably 0.2 to 2.0 mass%, and further preferably 0.5 to 1.5 mass%.
[0077] From the viewpoint of ensuring cement fluidity, the range of SO3 as the denominator of CL'SO3 / SO3 in condition (1), that is, the SO3 conversion amount of cement is preferably 3.5 mass % or less, more preferably 0.5 to 3.0 mass %, and further preferably 1.5 to 2.5 mass %.
[0078] [Condition (2)]
[0079] Condition (2) is that ΔC4AF is equal to or greater than 0.
[0080] In addition, the 0 point refers to a case where, for example, when C4AF (R.C4AF) obtained by Rietveld analysis is 10.1 mass %, C4AF (B.C4AF) calculated by Bauer's formula is also 10.1 mass %.
[0081] ΔC4AF represents the difference between the mass of R.C4AF and the mass of B.C4AF (R.C4AF-B.C4AF), and is the difference between C4AF (R.C4AF) obtained by Rietveld analysis and C4AF (B.C4AF) calculated by Baugh's formula. Since magnesium is not considered in Baugh's formula, the solid solution amount of MgO can be estimated based on ΔC4AF. If the MgO content in cement increases, ΔC4AF also increases. In the present invention, from the viewpoint of improving the long-term strength of mortar under high MgO conditions, ΔC4AF is set to be 0 or more.
[0082] Since the increase in the amount of ferrite phase in which MgO is solid-dissolved by the alkanolamine affects the strength improvement, ΔC4AF is preferably 0.3 to 1.5 points, and more preferably 0.5 to 1.5 points.
[0083] R.C4AF is calculated by the following steps.
[0084] First, the X-ray diffraction measurement of cement is carried out to obtain a curve. The obtained curve is analyzed by the Rietveld method, and the cement minerals are quantified. The minerals to be analyzed are set as C3S-M1 (M1 phase), C3S-M3 (M3 phase), C2S-α'H (α'H phase), C2S-β (β phase), C3A-cubic (cubic crystal), C3A-ortho (orthorhombic crystal), and C4AF. In the Rietveld analysis, based on the basic crystal structure data of each mineral, the lattice constant, proportional factor, etc. are used as parameters to perform a precision operation to fit the measured curve with the theoretical curve. Finally, based on the refined proportional factor, the mass ratio of the above-mentioned minerals is calculated, and the content (mass %) of R.C4AF is obtained.
[0085] Specific measurement conditions of the X-ray diffraction apparatus are shown in Examples.
[0086] The silicate cement in the present invention is not particularly limited as long as it satisfies the conditions (1) and (2) described above. It is also possible to use a blended cement obtained by mixing ordinary, early strength, super early strength, white, sulfate-resistant, medium heat, low heat, etc. silicate cement, blast furnace slag, fly ash, silica mixed materials (volcanic ash), etc., and alumina cement and other special cements. However, cement having a ferrite phase of 6% by mass or more in the Bauer formula is particularly preferred.
[0087] More specifically, the silicate cement used in the cement composition of the present invention is preferably ordinary silicate cement having a C3S (3CaO·SiO2) of 45 to 75 mass%, a C2S (2CaO·SiO2) of 5 to 25 mass%, a C3A (3CaO·Al2O3) of 7 to 11 mass%, and a C4AF (4CaO·Al2O3·Fe2O3) of 7 to 11 mass%, as calculated by the Bogle's formula.
[0088] Furthermore, in the Portland cement used in the cement composition of the present invention, C4AF (R.C4AF) obtained by Rietveld analysis is preferably 7.5 to 12% by mass.
[0089] (C3S, C2S)
[0090] The content of C3S in cement is 45% by mass or more, and thus the strength enhancement effect produced by adding alkanolamine is large, the mortar strength is excellent, and the fluidity is excellent. The content of C3S in cement is 45% by mass or more, and thus the content of C2S with relatively poor crushing property is reduced. As a result, the grinding time required for the cement composition to reach a constant Blaine specific surface area is shortened, and the excessive grinding of minerals (C3S, C3A and C4AF) other than C2S with good crushing property is mainly suppressed, and the increase of Blaine specific surface area is suppressed. In addition, regarding the mechanism of improving strength by adding alkanolamine, by selectively dissolving C4AF in clinker, the contact opportunity of C4AF close to C4AF with water is increased, and hydration is promoted, thereby improving strength. By suppressing excessive grinding of clinker, clinker particles in which each mineral exists in combination are difficult to exist as a single mineral, and the dissolution of C4AF easily promotes the hydration of C4AF, so it is easy to obtain the strength enhancement effect produced by adding alkanolamine.
[0091] The long-term compressive strength of concrete can be sufficiently maintained by setting the C3S content in cement to 75% by mass or less.
[0092] The long-term compressive strength of concrete can be sufficiently maintained by setting the C2S content in cement to 5% by mass or more.
[0093] When the C2S content in cement is 25% by mass or less, the initial compressive strength of concrete can be sufficiently maintained.
[0094] From the viewpoint of improving strength and fluidity, the C3S content in cement is more preferably 50 to 70% by mass.
[0095] (C4AF, C3A)
[0096] The content of C4AF in cement is 7% by mass or more, and thus the addition of alkanolamine promotes the dissolution of C4AF and the reaction of C3S, thereby achieving a significant strength-improving effect.
[0097] The C4AF content in cement is 11% by mass or less, thereby suppressing the amount of iron hydroxide gel generated by the dissolution of Fe ions in C4AF, suppressing the coating of the clinker particle surface, and thus preventing the delay of hydration.
[0098] The total content of C4AF and C3A is constant at about 18 mass %. If the content of C4AF in cement increases, the content of C3A decreases, and if the content of C4AF decreases, the content of C3A increases.
[0099] From the viewpoint of improving strength and fluidity, the content of C4AF in cement is preferably 7 to 9% by mass, more preferably 8 to 9% by mass.
[0100] 〔Alkanolamine〕
[0101] The cement composition of the present invention contains 0.001 to 0.025 parts by mass of alkanolamine based on 100 parts by mass of the Portland cement clinker in the present invention.
[0102] Alkanolamines also function as strength enhancers.
[0103] If the content of alkanolamine in the cement composition of the present invention is less than 0.001 parts by mass relative to 100 parts by mass of Portland cement clinker, the strength enhancement effect cannot be obtained. If the content of alkanolamine in the cement composition of the present invention exceeds 0.025 parts by mass relative to 100 parts by mass of Portland cement clinker, the initial strength enhancement effect is significant, but during the 28-day period, the initial hydration activity is active, resulting in a coarsening of the hydrated structure, thereby failing to obtain a strength enhancement effect.
[0104] From the above viewpoints, the content of the alkanolamine in the cement composition of the present invention is preferably 0.005 to 0.02 parts by mass relative to 100 parts by mass of the Portland cement clinker in the present invention.
[0105] Examples of the alkanolamine include monoethanolamine, diethanolamine, triethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, methylethanolamine, methylisopropanolamine, N-n-butylethanolamine, N-methyldiethanolamine, N-n-butyldiethanolamine, N-methyldiisopropanolamine, diethanolisopropanolamine, diisopropanolethanolamine, tetrahydroxyethylethylenediamine, N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine, and tris(2-hydroxybutyl)amine.
[0106] The alkanolamines may be used alone or in combination of two or more.
[0107] Among them, the alkanolamine is preferably at least one selected from the group consisting of diethanolisopropanolamine (DEIPA), triisopropanolamine (TIPA), ethanoldiisopropanolamine (EDIPA), triethanolamine (TEA), N-methyldiethanolamine (MDEA) and N-n-butyldiethanolamine (BDEA), more preferably at least one selected from the group consisting of diethanolisopropanolamine (DEIPA), triisopropanolamine (TIPA), ethanoldiisopropanolamine (EDIPA) and triethanolamine (TEA), and further preferably diethanolisopropanolamine (DEIPA).
[0108] Alkanolamines are generally high in viscosity and difficult to mix, and are not suitable for addition when producing mortar. Therefore, they are preferably added as a grinding aid in the final processing step of cement production. In addition, if the alkanolamine is diluted and dissolved in water for use, it is easy to mix with cement, and the cement composition of the present invention can be efficiently produced.
[0109] 〔plaster〕
[0110] The cement composition of the present invention contains gypsum.
[0111] As the gypsum, any of anhydrous gypsum, hemihydrate gypsum, and dihydrate gypsum can be used.
[0112] The content of gypsum in the cement composition is preferably 0.5 to 2.5% by mass in terms of SO 3 .
[0113] When the content of gypsum in the cement composition is within the above range, the drying shrinkage of the cement composition can be appropriately controlled, and the strength exhibited by the cement composition can be increased.
[0114] From the above viewpoints, the content of gypsum in the cement composition is more preferably 1.0 to 1.8% by mass in terms of SO 3 .
[0115] The ratio of SO3 in gypsum can be measured according to JIS R 5202:2010 "Chemical analysis methods for Portland cement". The ratio of the mass of gypsum in the cement composition converted into SO3 can be calculated from the amount of gypsum blended and the ratio of SO3 contained in the gypsum.
[0116] 〔limestone〕
[0117] The cement composition of the present invention may contain limestone for the purpose of improving short-term strength and reducing CO2 emissions by micronization.
[0118] The content of limestone in the cement composition is specified by JIS R 5210:2009 "Portland cement", but in the present invention, limestone may be added in an amount exceeding the range specified in the JIS standard.
[0119] The content of limestone in the cement composition is preferably 0 to 20% by mass, more preferably 0 to 10% by mass, and further preferably 2 to 5% by mass. In addition, a content of limestone of 0% by mass means that limestone is not added during the production of the cement composition.
[0120] [Other ingredients]
[0121] Fly ash, blast furnace slag, microsilica powder, etc. may be added to the cement composition of the present invention in order to adjust fluidity, hydration rate, strength development, etc.
[0122] (Blaine specific surface area)
[0123] The Blaine specific surface area of the cement composition of the present invention is preferably 3000 to 3400 cm 2 / g.
[0124] The specific surface area of the Blaine is 3000cm 2 / g or more, the mortar strength is not easy to reduce, through 3400cm 2 / g or less, the decrease in fluidity can be suppressed, and the decrease in dissolution of C4AF by alkanolamine can be suppressed, thereby maintaining the strength improvement effect.
[0125] From the viewpoint of further improving strength, the Blaine specific surface area of the cement composition is more preferably 3100 to 3300 cm 2 / g.
[0126] The Blaine specific surface area of the cement composition may be measured in accordance with JIS R 5201:2015 “Physical testing methods for cement”.
[0127] <Method for producing cement composition>
[0128] The method for producing a cement composition of the present invention is a method for producing the cement composition of the present invention by mixing silicate cement and alkanolamine, wherein the silicate cement satisfies the following (1) and (2), and the alkanolamine is 0.001 to 0.025 parts by mass based on 100 parts by mass of the silicate cement.
[0129] (1)0.55≤MgO / Fe2O3+CL'SO3 / SO3≤0.95
[0130] (2) 0≤ΔC4AF
[0131] In (1), MgO represents the mass (mass %) of MgO in Portland cement, Fe2O3 represents the mass (mass %) of Fe2O3 in Portland cement, SO3 represents the SO3 equivalent amount (mass %) of Portland cement, and CL'SO3 represents the SO3 equivalent amount (mass %) of Portland cement clinker.
[0132] In (2), ΔC4AF represents the difference between the mass (mass %) of R.C4AF and the mass (mass %) of B.C4AF (R.C4AF-B.C4AF). R.C4AF represents the C4AF value of silicate cement measured by a powder X-ray diffraction device, and B.C4AF represents 3.04×Fe2O3. Fe2O3 in B.C4AF represents the mass (mass %) of Fe2O3 in silicate cement.
[0133] The silicate cement used in the method for producing the cement composition of the present invention is the same as the silicate cement contained in the cement composition of the present invention, and the preferred embodiment is also the same. That is, MgO / Fe2O3 is preferably greater than 0.35, and the silicate cement in the present invention is preferably ordinary silicate cement having C3S of 45 to 75% by mass, C2S of 5 to 25% by mass, C3A of 7 to 11% by mass, and C4AF of 7 to 11% by mass as calculated by the Bogle formula.
[0134] The amount of alkanolamine added is the same as the content of alkanolamine in the cement composition of the present invention, and the preferred range is also the same. That is, the amount of alkanolamine added is preferably 0.005 to 0.02 parts by mass per 100 parts by mass of the Portland cement in the present invention.
[0135] Furthermore, the amount of limestone blended is the same as the above-mentioned limestone content, and the preferred range is also the same.
[0136] The alkanolamine used in the method for producing the cement composition of the present invention is the same as the alkanolamine contained in the cement composition of the present invention, and the preferred aspects are also the same.
[0137] That is, the alkanolamine used in the method for producing the cement composition of the present invention is preferably at least one selected from the group consisting of diethanolisopropanolamine, triisopropanolamine, ethanoldiisopropanolamine, triethanolamine, N-methyldiethanolamine, and N-n-butyldiethanolamine.
[0138] Alkanolamines are generally high in viscosity and difficult to mix, and are not suitable for addition when producing mortar. Therefore, they are preferably added as a grinding aid in the final processing step of cement production. In addition, if the alkanolamine is diluted and dissolved in water for use, it is easy to mix with cement, and the cement composition of the present invention can be efficiently produced.
[0139] The mixing mechanism of each component in the manufacturing method of the cement composition of the present invention is not particularly limited. For example, a mixer, a ball mill, a Roche mill, an air mixing cyclone separator, etc. can be cited. The mixing time can be set within the range determined to be fully mixed in the manufacture of the conventional cement composition.
[0140] In the present production method, it is preferred that the Blaine specific surface area of the cement composition be 3000 to 3400 cm 2 / g method for crushing.
[0141] In the method for producing the cement composition of the present invention, in addition to the silicate cement clinker, gypsum, limestone and alkanolamine of the present invention, blast furnace slag, siliceous admixture and fly ash may be further added.
[0142] In the present invention, blast furnace slag and silica mixed materials specified in JIS R 5210: 2009 "Portland Cement" can be used. As for fly ash, in addition to fly ash type I and fly ash type II specified in JIS R 5210: 2009 "Portland Cement", fly ash type III and fly ash type IV can also be used.
[0143] Example
[0144] Hereinafter, the present invention will be described in further detail with reference to Examples, but the present invention is not limited to the following Examples.
[0145] <Components of cement composition>
[0146] The following materials were used in the production of the cement composition.
[0147] 1. Clinker
[0148] Ordinary Portland cement clinker (manufactured by SUMITOMOOSAKA CEMENT Co., Ltd.) having the chemical composition and mineral composition shown in Tables 1 and 2 was used. In Tables 1 and 2, HM refers to hydraulic modulus, SM refers to silica modulus, and IM refers to iron modulus. In addition, "%" in Tables 1 and 2 is a mass basis (mass %).
[0149] The chemical composition of the clinker was analyzed by the glass bead method using a fluorescent X-ray analyzer (PRIMUS IV, manufactured by Rigaku Corporation) in accordance with JIS R 5204:2019 "Fluorescent X-ray analysis of cement". The mineral composition was calculated using the following Bauer's formula based on the mass ratios of CaO, SiO2, Al2O3, and Fe2O3 obtained.
[0150] C3S=(4.07×CaO)-(7.60×SiO2)-(6.72×Al2O3)-(1.43×Fe2O3)
[0151] C2S=(2.87×SiO2)-(0.754×C3S)
[0152] C3A=(2.65×Al2O3)-(1.69×Fe2O3)
[0153] C4AF=3.04×Fe2O3
[0154] (Chemical and mineralogical composition of clinker)
[0155] The chemical composition and mineral composition of the clinker are shown in Tables 1 and 2.
[0156] [Table 1]
[0157]
[0158] [Table 2]
[0159]
[0160] 2. Alkanolamines
[0161] ·DEIPA: Diethanol isopropanolamine (manufactured by Tokyo Chemical Industry Co., Ltd.) ·TEA: Triethanolamine (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0162] TIPA: Triisopropanolamine (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0163] ·EDIPA: ethanol diisopropanolamine
[0164] [Made by Sigma-Aldrich Japan KK]
[0165] 3. Limestone
[0166] Made by KANTO KAGAKU., special grade calcium carbonate, CaCO3: 99.5%
[0167] 4. Plaster
[0168] Hemihydrate gypsum was used. Specifically, chemical gypsum (CaSO4 (97.8 mol%)) was kept in a dryer at 120°C for 12 hours. The SO3 conversion amount in the gypsum was measured according to JIS R5202:2015 "Chemical analysis of cement". The composition of the chemical gypsum is shown in Table 3.
[0169] [Table 3]
[0170] <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO <![CDATA[Fe2O3]]> <![CDATA[SO3]]> <![CDATA[TiO2]]> <![CDATA[P2O5]]> 0.19 0.48 31.94 2.19 47.76 0.29 0.12
[0171] (quality%)
[0172] <Manufacturing of cement>
[0173] The clinkers shown in Tables 1 and 2 were mixed in a mixer by adding limestone to 3.2% by mass in the obtained cement and adding gypsum (the above-mentioned hemihydrate gypsum) to the mixture shown in Table 4, thereby obtaining cement. In Table 4, CL represents clinker. And, "%" is based on mass.
[0174] [Table 4]
[0175]
[0176] (Chemical and mineral composition of cement)
[0177] The chemical composition of cement was measured by the same method as the chemical composition of clinker, and the mineral composition of cement was calculated by the same method as the mineral composition of clinker. The results are shown in Tables 5 to 9. In addition, "%" in Tables 5 to 9 is a mass basis (mass %).
[0178] In addition, the value of "C4AF" in Table 6 is B.C4AF in the present invention, and the value shown in the "Bauer" column in the "C4AF (%)" column in Tables 7 to 9 is reference. The value in the "Ritvold" column in the "C4AF (%)" column in Tables 7 to 9 is R.C4AF in the present invention, and is the C4AF value of cement measured by a powder X-ray diffraction device. Specifically, the measurement was performed under the following measurement conditions using the Rietvold analysis method using powder X-ray diffraction.
[0179] (Measurement conditions)
[0180] · Powder X-ray diffraction apparatus: PANalytical, X'Part Powder
[0181] Rietveld analysis software: PANalytical, X'Part HighScore Plus version 2.1b
[0182] X-ray tube: Cu (tube voltage: 45kV, tube current: 40mA)
[0183] Slit: Divergence slit - variable (irradiation width - 12mm, anti-scattering slit - 2°)
[0184] ·Measurement range: 2θ=10~70°(step length: 0.017°)
[0185] Scanning speed: 0.1012° / s
[0186] The ratio (mass %) of each mineral in cement was obtained using the analysis function based on the Rietveld method installed in the above software in accordance with the joint experimental procedure book 2 of the document "Report C-12 of the Cement Chemistry Expert Committee: Study on the Difference of Clinker Mineral Amounts Caused by Difference in Measurement Methods, Part 2, Chapter 4, Study on Quantification Based on Powder X-ray Diffraction / Ritveld Analysis". And, the total of the ratio of each mineral was set to 100 mass %, and the content R.C4AF (mass %) of C4AF in each Example and Comparative Example was obtained.
[0187] The "Δ" in the "C4AF (%)" column in Tables 7 to 9 * The value in the " " column represents the difference (R.C4AF-B.C4AF) between the value (B.C4AF) shown in the "Baugh" column in the "C4AF(%)" column in Tables 7 to 9 and the value (R.C4AF) shown in the "Ritvold" column in the "C4AF(%)" column in Tables 7 to 9.
[0188] and, Figure 1 The conditions for the examples and comparative examples are shown in FIG. ** Graph of the ΔC4AF values.
[0189] [Table 5]
[0190]
[0191] [Table 6]
[0192]
[0193] <Manufacturing of cement composition>
[0194] [Example 1]
[0195] As cement compositions to which no amine was added, cements shown in Tables 5 to 7 were used.
[0196] As cement compositions to which amines were added, compositions composed of the alkanolamines (DEIPA) shown in Table 7 and the cements shown in Tables 5 and 7 were prepared. Specifically, alkanolamines were mixed with cement in an amount such that the concentration of the alkanolamines in the total of cement and alkanolamines was 10 ppm (0.001 parts by mass relative to 100 parts by mass of cement).
[0197] Next, the cement composition without amine addition and the cement composition with amine addition were mixed and pulverized using a test ball mill so that the Blaine specific surface area value became 3300 cm 2 / g, thereby obtaining each cement composition of Example 1.
[0198] [Example 2 to Example 19, Comparative Example 1 to Comparative Example 7]
[0199] As cement compositions to which no amine was added, cements shown in Tables 5 to 8 were used.
[0200] A cement composition to which amine was added was obtained in the same manner as in Example 1 except that the cements shown in Tables 5 to 8 were used and DEIPA was used in an amount to give a concentration shown in Table 7 or 8 in the total of cement and DEIPA.
[0201] Next, the cement composition without amine addition and the cement composition with amine addition were mixed and pulverized using a test ball mill so that the Blaine specific surface area value became 3300 cm 2 / g, thereby obtaining each cement composition of Examples 2 to 19 and Comparative Examples 1 to 7.
[0202] [Example 20 to Example 22]
[0203] As cement compositions to which no amine was added, cements shown in Tables 5, 6, and 9 were used.
[0204] A cement composition to which an amine was added was obtained in the same manner as in Example 7 except that the alkanolamine listed in "Amine Type" in Table 9 was used instead of DEIPA.
[0205] Next, the cement composition without amine addition and the cement composition with amine addition were mixed and pulverized using a test ball mill so that the Blaine specific surface area value became 3300 cm 2 / g, thereby obtaining each cement composition of Example 20 to Example 22.
[0206] <Evaluation of cement composition>
[0207] Using the cement compositions to which no amine was added and the cement compositions to which amine was added of the respective Examples and Comparative Examples, test materials were prepared in accordance with "Physical Testing Methods for Cement" of JIS R 5201:2015, and mortar compressive strength tests were measured.
[0208] In addition, the mix ratio of the test material was 11.1 mass % of water, 66.7 mass % of aggregate, and 22.2 mass % of cement. The size of the test material was a rectangular parallelepiped of 40 mm×40 mm×160 mm. After the test material was made, it was wrapped and cured with a vinyl chloride resin.
[0209] The compressive strength of the mortar obtained using the cement composition without amine addition is shown in the "Age (without addition) (a)" column of Tables 7 to 9, and the compressive strength of the mortar obtained using the cement composition with amine addition is shown in the "Age (with amine addition) (b)" column of Tables 7 to 9. The larger the numerical value, the higher the compressive strength of the mortar.
[0210] The column "Δ(ba)" in Tables 7 to 9 shows the difference (strength difference) obtained by subtracting the compressive strength of the mortar obtained by using the cement composition to which amine is added from the compressive strength of the mortar obtained by using the cement composition to which amine is added. The larger the value of the strength difference, the greater the strength improvement effect.
[0211] and, Figure 2 The conditions for the 7-day and 28-day-old animals are shown in ** Here, the "condition ** " is the "condition" in Tables 7 to 9 ** The numerical values shown in the column "MgO / Fe2O3+CL'SO3 / SO3" of condition (1) of the silicate cement in the present invention.
[0212] [Table 7]
[0213]
[0214] [Table 8]
[0215]
[0216] [Table 9]
[0217]
[0218] The strength difference of the mortar shown in the "Δ(ba)" column of Tables 7 to 9 indicates how much the strength of the mortar obtained by using the cement composition with added amines is increased compared to the mortar obtained by using the cement composition without added amines. The larger the positive value is, the greater the strength enhancement effect is. If the results of the 3-day-old age are compared with the results of the 7-day-old age and the 28-day-old age, it can be seen that the values of Δ(ba) above 7 days old are large, and the strength enhancement effect is large. In addition, the comparison between the 7-day-old age and the 28-day-old age is as follows: Figure 2 As shown, it can be seen that the strength enhancement effect is large at 28 days of age.
Claims
1. A cement composition comprising: Portland cement satisfying the following (1) and (2); and alkanolamine, which is 0.001 to 0.025 parts by mass relative to 100 parts by mass of the silicate cement, The silicate cement is ordinary silicate cement having C3S of 45-75 mass %, C2S of 5-25 mass %, C3A of 7-11 mass %, and C4AF of 7-11 mass % calculated by Bauer's formula. (1)0.55≤MgO / Fe2O3+CL'SO3 / SO3≤0.95 (2) 0≤ΔC4AF In (1), MgO represents the mass of MgO in the silicate cement, Fe2O3 represents the mass of Fe2O3 in the silicate cement, SO3 represents the SO3-converted amount of the silicate cement, CL'SO3 represents the SO3-converted amount of the clinker of the silicate cement, In (2), ΔC4AF represents the difference between the mass of R.C4AF and the mass of B.C4AF, i.e., R.C4AF-B.C4AF, where The R.C4AF represents the C4AF value of the silicate cement measured by a powder X-ray diffraction device, the B.C4AF represents 3.04×Fe2O3, and the Fe2O3 in the B.C4AF represents the mass of Fe2O3 in the silicate cement. The masses and converted amounts referred to in (1) and (2) above are expressed in mass %.
2. The cement composition according to claim 1, wherein In (1), the MgO / Fe2O3 exceeds 0.
35.
3. The cement composition according to claim 1 or 2, wherein: The content of the alkanolamine is 0.005 to 0.02 parts by mass relative to 100 parts by mass of the silicate cement.
4. The cement composition according to claim 1 or 2, wherein The alkanolamine is at least one selected from the group consisting of diethanolisopropanolamine, triisopropanolamine, ethanoldiisopropanolamine, triethanolamine, N-methyldiethanolamine, and N-n-butyldiethanolamine.
5. The cement composition according to claim 3, wherein The alkanolamine is at least one selected from the group consisting of diethanolisopropanolamine, triisopropanolamine, ethanoldiisopropanolamine, triethanolamine, N-methyldiethanolamine, and N-n-butyldiethanolamine.
6. A method for producing a cement composition, wherein: Portland cement and alkanolamine are mixed, wherein the Portland cement satisfies the following (1) and (2), and the alkanolamine is 0.001 to 0.025 parts by mass based on 100 parts by mass of the Portland cement. The silicate cement is ordinary silicate cement having C3S of 45-75 mass %, C2S of 5-25 mass %, C3A of 7-11 mass %, and C4AF of 7-11 mass % calculated by Bauer's formula. (1)0.55≤MgO / Fe2O3+CL'SO3 / SO3≤0.95 (2) 0≤ΔC4AF In (1), MgO represents the mass of MgO in the silicate cement, Fe2O3 represents the mass of Fe2O3 in the silicate cement, SO3 represents the SO3-converted amount of the silicate cement, CL'SO3 represents the SO3-converted amount of the clinker of the silicate cement, In (2), ΔC4AF represents the difference between the mass of R.C4AF and the mass of B.C4AF, i.e., R.C4AF-B.C4AF, wherein R.C4AF represents the C4AF value of the silicate cement measured by a powder X-ray diffraction device, B.C4AF represents 3.04×Fe2O3, and Fe2O3 in B.C4AF represents the mass of Fe2O3 in the silicate cement. The masses and converted amounts referred to in (1) and (2) above are expressed in mass %.
7. The method for producing a cement composition according to claim 6, wherein: In (1), the MgO / Fe2O3 exceeds 0.
35.
8. The method for producing a cement composition according to claim 6 or 7, wherein: The amount of the alkanolamine added is 0.005 to 0.02 parts by mass relative to 100 parts by mass of the silicate cement.
9. The method for producing a cement composition according to claim 6 or 7, wherein: The alkanolamine is at least one selected from the group consisting of diethanolisopropanolamine, triisopropanolamine, ethanoldiisopropanolamine, triethanolamine, N-methyldiethanolamine, and N-n-butyldiethanolamine.
10. The method for producing a cement composition according to claim 8, wherein: The alkanolamine is at least one selected from the group consisting of diethanolisopropanolamine, triisopropanolamine, ethanoldiisopropanolamine, triethanolamine, N-methyldiethanolamine, and N-n-butyldiethanolamine.