Aqueous polyurethane composition and production method thereof

Through a water-based polyurethane production method that does not require organic solvents, the problems of environmental pollution and low solid content in the existing technology are solved, and a water-based polyurethane composition with high solid content and good mechanical properties is achieved, with good tensile strength and solvent resistance. .

CN118184943BActive Publication Date: 2024-10-01SHENGDING HIGHTECH MATERIALS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410376867.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2024-10-01
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

The existing preparation method of water-based polyurethane requires the use of organic solvents, resulting in environmental pollution and low solid content, and the resulting product has insufficient tensile strength and bonding strength.

Method used

Using a production method that does not require the use of organic solvents, the polymer diol is reacted with a diisocyanate and a catalyst to form a prepolymer, followed by reaction with a hydrophilic chain extender and neutralizing agent, and an emulsification step to form an aqueous polyurethane composition, and finally Chain extension with specific compounds to obtain water-based polyurethane with high solid content and low viscosity.

Benefits of technology

It achieves high solid content, good mechanical properties and solvent resistance, and the cured water-based polyurethane has high tensile strength and bonding strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004767296060000021
    Figure BDA0004767296060000021
  • Figure BDA0004767296060000031
    Figure BDA0004767296060000031
  • Figure BDA0004767296060000032
    Figure BDA0004767296060000032
Patent Text Reader

Abstract

The present invention discloses an aqueous polyurethane composition and a production method thereof, comprising the following steps: (1) treating a polymer diol at 100-150°C for 0.5-5h to obtain a dehydrated diol; cooling the dehydrated diol to a temperature of ≤70°C, and then adding a diisocyanate and a catalyst to the cooled diol to obtain a prepolymer; (2) reacting the prepolymer with a hydrophilic chain extender and a neutralizer to obtain an intermediate; (3) emulsifying the intermediate, 20-40 parts by weight of water and 0.5-3 parts by weight of sodium polyoxyethylene alcohol carboxylate to obtain an intermediate emulsion; emulsifying the intermediate emulsion with 60-85 parts by weight of water to obtain an emulsified product; (4) reacting the emulsified product, 3-8 parts by weight of a first compound and 1.5-4 parts by weight of a second compound to obtain an aqueous polyurethane composition. The method does not require the use of an organic solvent during the production process, and the obtained product has a high solid content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an aqueous polyurethane composition and a production method thereof. Background Art

[0002] Waterborne polyurethane has the advantages of being non-toxic, non-flammable, and having no irritating odor, and is widely used in various fields. At present, the preparation methods of waterborne polyurethane mainly include solution method and prepolymer mixing method. Solution method refers to preparing a high molecular weight polyurethane solution containing hydrophilic groups in an inert solvent with a low boiling point and miscible with water, and then diluting the solution with water to form an emulsion with an oil-in-water solvent as a continuous phase. A large amount of water is added to the above emulsion to make it phase inverted, becoming a dispersion with water as a continuous phase, and removing the solvent to obtain waterborne polyurethane. Prepolymer mixing method avoids the large amount of solvent required in solution method, which first polymerizes isocyanate and polyol bulk to form prepolymer, and then uses a small amount of solvent to dilute the prepolymer and then chain extend and emulsify to obtain waterborne polyurethane. It can be seen that both solution method and prepolymer mixing method need to use organic solvents, so that volatile organic compounds will be released during the preparation process, polluting the environment. In addition, the solid content of waterborne polyurethane obtained by the above method is relatively low.

[0003] CN116813870A discloses a method for preparing an aqueous polyurethane resin dispersion, which comprises mixing isophorone diisocyanate and polytetrahydrofuran ether diol, introducing nitrogen, adding a catalyst, stirring and mixing at room temperature, heating to 50-60°C for reaction for 1-2 hours, and further heating to 70-80°C for reaction for 0.5-1 hour to obtain a polyurethane prepolymer. Antibacterial silicone oil and a small molecule chain extender are added to the polyurethane prepolymer, and the temperature is further raised to 80-85°C for reaction for 5-8 hours, and further reacted for 3-5 hours, and then cooled to 40-45°C and a neutralizer is added. After reacting for 1-2 hours, deionized water and antioxidant graphite phase desalination carbon are added, and the mixture is stirred at high speed and naturally defoamed to obtain an aqueous polyurethane resin dispersion. The aqueous polyurethane resin dispersion obtained by the preparation method has a low tensile strength.

[0004] CN116333262A discloses a method for preparing a solvent-free waterproof and breathable waterborne polyurethane dispersion, wherein a polyether polyol is reacted with a polyisocyanate to obtain a prepolymer; a chain extender and water are sequentially added to the prepolymer and mixed to obtain a solvent-free waterproof and breathable waterborne polyurethane dispersion. The solid content of the polyurethane dispersion is low and the mechanical properties need to be improved. Summary of the invention

[0005] In view of this, one object of the present invention is to provide a method for producing an aqueous polyurethane composition, wherein no organic solvent is required during the production process, and the obtained product has a high solid content. Furthermore, the polyurethane composition obtained by the production method has a low viscosity, and after curing, it has good mechanical properties, bonding strength and solvent resistance. Another object of the present invention is to provide an aqueous polyurethane composition.

[0006] In one aspect, the present invention provides a method for producing an aqueous polyurethane composition, comprising the steps of:

[0007] (1) treating a polymer diol as represented by formula (I) at 100 to 150° C. for 0.5 to 5 h to obtain a dehydrated diol; cooling the dehydrated diol to a temperature of ≤70° C., and then adding a diisocyanate as represented by formula (II) and a catalyst to the cooled diol to obtain a prepolymer;

[0008]

[0009] In formula (I), R 5 An alkylene group selected from C1 to C6, wherein n represents the degree of polymerization; the molecular weight of the polymer diol is 500 to 4000;

[0010]

[0011] In formula (II), R 1 ~R 3 R are independently selected from H, C1-C6 alkyl; 4 An alkylene group selected from C1 to C6;

[0012] (2) reacting the prepolymer with a hydrophilic chain extender and a neutralizer to obtain an intermediate;

[0013] (3) emulsifying the intermediate, 20 to 40 parts by weight of water and 0.5 to 3 parts by weight of sodium fatty alcohol polyoxyethylene ether carboxylate to obtain an intermediate emulsion; and emulsifying the intermediate emulsion with 60 to 85 parts by weight of water to obtain an emulsified product;

[0014] (4) reacting the emulsified product, 3 to 8 parts by weight of a first compound represented by formula (III), and 1.5 to 4 parts by weight of a second compound represented by formula (IV) to obtain an aqueous polyurethane composition;

[0015]

[0016] In formula (III), R 7 ~R 9 are independently selected from H or C1-C6 alkyl, R 6 An alkylene group selected from C1 to C6;

[0017]

[0018] In formula (IV), R 10 ~R 12 Each of them is independently selected from a C1-C6 alkyl group, x is selected from an integer of 1-6, and y is selected from an integer of 1-6.

[0019] According to the production method of the present invention, preferably, the catalyst is a metal carboxylate; the metal element in the metal carboxylate is selected from one or more of bismuth and zinc; the metal carboxylate is selected from one or more of neocaprylate, isooctanoate and laurate.

[0020] According to the production method of the present invention, preferably, the amount of polymer diol used is 40 to 70 parts by weight, the amount of diisocyanate used is 15 to 35 parts by weight, and the amount of catalyst used is 0.02 to 0.2 parts by weight.

[0021] According to the production method of the present invention, preferably, in step (1), the reaction temperature is 70 to 100° C. and the reaction time is 1 to 5 hours.

[0022] According to the production method of the present invention, preferably, the aqueous chain extender is selected from one or more of dimethylolpropionic acid, dimethylolbutyric acid, N-methyldiethanolamine, bis-2-hydroxyethylbenzylamine, and bis-2-hydroxypropylbenzylamine;

[0023] The neutralizing agent is selected from one or more of triethylamine, tripropylamine, tributylamine, dimethylcyclohexylamine, formic acid, acetic acid, hydrochloric acid, sodium hydroxide, and epichlorohydrin.

[0024] According to the production method of the present invention, preferably, the amount of the hydrophilic chain extender is 2 to 9 parts by weight, and the amount of the neutralizer is 0.5 to 4 parts by weight.

[0025] According to the production method of the present invention, preferably, the reaction temperature of step (2) is 45-75° C., and the reaction time is 0.5-4 h.

[0026] According to the production method of the present invention, preferably, the time of the first emulsification is 1 to 8 minutes, and the time of the second emulsification is 5 to 20 minutes.

[0027] According to the production method of the present invention, preferably, the polymer diol is polycaprolactone diol, the diisocyanate is isophorone diisocyanate, the first compound is isophorone diamine, and the second compound is N-2-aminoethyl-3-aminopropyltriethoxysilane.

[0028] On the other hand, the present invention provides an aqueous polyurethane composition, which is obtained by the above production method, and the solid content of the aqueous polyurethane composition is ≥45wt%.

[0029] The production method of the present invention does not require the use of organic solvents during the production process, and the obtained product has a high solid content. Furthermore, the polyurethane composition obtained by the production method has a low viscosity, and after curing, it has good mechanical properties, bonding strength and solvent resistance. DETAILED DESCRIPTION

[0030] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0031] <Method for producing aqueous polyurethane composition>

[0032] The method for producing the aqueous polyurethane composition of the present invention comprises the following steps: (1) obtaining a prepolymer; (2) obtaining an intermediate; (3) emulsifying; and (4) further chain extension. The method is described in detail below.

[0033] Steps to obtain prepolymer

[0034] The invention treats the polymer diol at 100-150°C for 0.5-5h to obtain dehydrated diol; cools the dehydrated diol to a temperature of ≤70°C, and then adds diisocyanate and a catalyst to the cooled diol to obtain a prepolymer.

[0035] The polymer diol is shown in formula (I):

[0036]

[0037] In formula (I), R 5 The alkylene group is selected from C1 to C6, and n represents the degree of polymerization; the molecular weight of the polymer diol is 500 to 4000.

[0038] Preferably, R 5 is selected from C2 to C5 alkylene; more preferably, R 5 An alkylene group selected from C3 to C4.

[0039] The molecular weight of the polymer diol is preferably 1,000 to 3,000; more preferably 1,500 to 2,500.

[0040] In certain embodiments, the polymer diol is polycaprolactone diol.

[0041] Preferably, the polymer diol is treated at 120-140°C for 1-4 hours; more preferably, the polymer diol is treated at 120-130°C for 2-3 hours. The above treatment steps can be carried out under vacuum conditions. Vacuum can refer to a pressure of ≤10Pa; preferably, a pressure of ≤1Pa; more preferably, a pressure of ≤10 -1 Pa.

[0042] Preferably, the dehydrated glycol is cooled to a temperature of 15 to 60° C. More preferably, the dehydrated glycol is cooled to a temperature of 40 to 60° C. The dehydrated glycol may be cooled in an inert gas atmosphere.

[0043] The amount of the polymer diol used is 40 to 70 parts by weight, preferably 45 to 65 parts by weight, and more preferably 50 to 60 parts by weight.

[0044] The diisocyanate is shown in formula (II):

[0045]

[0046] In formula (II), R 1 ~R 3 R are independently selected from H, C1-C6 alkyl; 4 An alkylene group selected from C1 to C6.

[0047] Preferably, R 1 ~R 3 R are independently selected from H, C1-C3 alkyl; 4 is selected from C1 to C3 alkylene. More preferably, R 1 ~R 3 are independently selected from C1-C2 alkyl groups; R 4 An alkylene group selected from C1 to C2.

[0048] According to one embodiment of the present invention, the diisocyanate is isophorone diisocyanate.

[0049] The amount of diisocyanate used is 15 to 35 parts by weight, preferably 20 to 30 parts by weight, and more preferably 25 to 28 parts by weight.

[0050] The catalyst may be a metal carboxylate. The metal element in the metal carboxylate may be selected from one or more of bismuth and zinc. The metal carboxylate may be selected from one or more of neodecanoate, isooctanoate, and laurate. Examples of the catalyst include, but are not limited to, bismuth neodecanoate, bismuth isooctanoate, bismuth laurate, zinc neodecanoate, zinc laurate, and zinc isooctanoate. According to one embodiment of the present invention, the catalyst is bismuth isooctanoate.

[0051] The amount of the catalyst used may be 0.02 to 0.2 parts by weight; preferably 0.05 to 0.15 parts by weight; more preferably 0.08 to 0.1 parts by weight.

[0052] The reaction temperature may be 70 to 100°C; preferably 80 to 95°C; more preferably 85 to 90°C.

[0053] The reaction time may be 1 to 5 hours, preferably 2 to 4 hours, and more preferably 3 to 3.5 hours.

[0054] The reaction can be carried out under stirring.

[0055] Steps to obtain intermediates

[0056] The prepolymer is reacted with a hydrophilic chain extender and a neutralizing agent to obtain an intermediate.

[0057] In certain embodiments, the prepolymer is cooled to 10-60°C; preferably, to 20-50°C; more preferably, to 30-40°C, and then a hydrophilic extender and a neutralizer are added to the cooled prepolymer.

[0058] The hydrophilic chain extender can be selected from one or more of dimethylol propionic acid, dimethylol butyric acid, N-methyldiethanolamine, bis-2-hydroxyethyl benzylamine, and bis-2-hydroxypropyl benzylamine. Preferably, the hydrophilic chain extender is dimethylol butyric acid.

[0059] The amount of the hydrophilic chain extender can be 2 to 9 parts by weight, preferably 3 to 8 parts by weight, and more preferably 4 to 6 parts by weight.

[0060] The neutralizing agent can be selected from one or more of triethylamine, tripropylamine, tributylamine, dimethylcyclohexylamine, formic acid, acetic acid, hydrochloric acid, sodium hydroxide, and epichlorohydrin. Preferably, the neutralizing agent is triethylamine.

[0061] The amount of the neutralizer used may be 0.5 to 4 parts by weight, preferably 1 to 3 parts by weight, and more preferably 1.5 to 2 parts by weight.

[0062] The reaction temperature may be 45 to 75°C; preferably 50 to 70°C; more preferably 60 to 65°C.

[0063] The reaction time may be 0.5 to 4 hours; preferably 1 to 3 hours; more preferably 2 to 2.5 hours.

[0064] Emulsification steps

[0065] The intermediate, 20-40 parts by weight of water and 0.5-3 parts by weight of sodium polyoxyethylene alcohol ether carboxylate are emulsified once to obtain an intermediate emulsion; the intermediate emulsion is emulsified twice with 60-85 parts by weight of water to obtain an emulsified product.

[0066] In the primary emulsification, the amount of water used is 20 to 40 parts by weight, preferably 25 to 35 parts by weight, and more preferably 30 to 32 parts by weight.

[0067] The amount of sodium fatty alcohol polyoxyethylene ether carboxylate used is 0.5 to 3 parts by weight, preferably 1 to 2.5 parts by weight, and more preferably 1.5 to 2 parts by weight.

[0068] The primary emulsification time may be 1 to 8 minutes, preferably 2 to 7 minutes, and more preferably 4 to 5 minutes.

[0069] In certain embodiments, water is added to the intermediate emulsion at a temperature of 10 to 38°C; preferably 15 to 30°C; more preferably 20 to 25°C.

[0070] In the secondary emulsification, the amount of water used is 60 to 85 parts by weight, preferably 65 to 80 parts by weight, and more preferably 70 to 75 parts by weight.

[0071] The secondary emulsification time may be 5 to 20 minutes, preferably 7 to 15 minutes, and more preferably 10 to 12 minutes.

[0072] Steps to further chain expansion

[0073] The emulsified product, 3 to 8 parts by weight of the first compound and 1.5 to 4 parts by weight of the second compound are reacted to obtain an aqueous polyurethane composition.

[0074] The first compound is represented by formula (III):

[0075]

[0076] In formula (III), R 7 ~R 9 are independently selected from H or C1-C6 alkyl, R 6 An alkylene group selected from C1 to C6.

[0077] Preferably, R 7 ~R 9 are independently selected from H or C1-C3 alkyl; more preferably, R 7 ~R 9 Each is independently selected from a C1-C2 alkyl group.

[0078] Preferably, R 6 is selected from C1 to C3 alkylene; more preferably, R 6 An alkylene group selected from C1 to C2.

[0079] According to one embodiment of the present invention, the first compound is isophoronediamine.

[0080] The amount of the first compound used is 3 to 8 parts by weight, preferably 4 to 7 parts by weight, and more preferably 5 to 6 parts by weight.

[0081] The second compound is represented by formula (IV):

[0082]

[0083] In formula (IV), R 10 ~R 12 Each of them is independently selected from a C1-C6 alkyl group, x is selected from an integer of 1-6, and y is selected from an integer of 1-6.

[0084] Preferably, R 10 ~R 12 are independently selected from C2 to C5 alkyl groups; more preferably, R 10 ~R 12 are independently selected from C2 to C3 alkyl groups. 10 ~R 12 All are ethyl.

[0085] Preferably, x is selected from an integer of 2-5; more preferably, x is selected from an integer of 3-4.

[0086] Preferably, y is selected from an integer of 1-4; more preferably, y is selected from an integer of 1-2.

[0087] The amount of the second compound used is 1.5 to 4 parts by weight, preferably 2 to 3 parts by weight, and more preferably 2.5 to 3 parts by weight.

[0088] The reaction temperature may be 15 to 35°C; preferably 20 to 30°C; more preferably 20 to 25°C.

[0089] The reaction time may be 0.5 to 3 hours, preferably 1 to 3 hours, and more preferably 1 to 2 hours.

[0090] <Aqueous polyurethane composition>

[0091] The solid content of the aqueous polyurethane composition is ≥45 wt %; preferably, the solid content is ≥48 wt %. The solid content can be determined by the method specified in BS EN ISO 3251-2019 Determination of non-volatile matter content of paints, varnishes and plastics.

[0092] The viscosity of the aqueous polyurethane composition is 400 to 600 cP, preferably 450 to 550 cP, and more preferably 480 to 500 cP. The viscosity can be obtained by measuring the melt viscosity at 25° C. using a Brookfield DV2T rotary viscometer.

[0093] The tensile strength of the aqueous polyurethane composition is ≥50 MPa; preferably, the tensile strength is ≥54 MPa. In certain embodiments, the tensile strength is 54-56 MPa.

[0094] The elongation of the waterborne polyurethane composition is ≥500%; preferably, the elongation is ≥550%; more preferably, the elongation is 580-600%.

[0095] The 100% modulus of the waterborne polyurethane composition is ≥7 MPa; preferably, the 100% modulus is ≥9 MPa. In certain embodiments, the 100% modulus is 9.2-9.5 MPa.

[0096] The tensile strength, elongation and 100% modulus of tensile strength can be determined by the method specified in GB / T528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber.

[0097] The bonding strength of the waterborne polyurethane composition is ≥55 N; preferably, the bonding strength is ≥60 N. In some embodiments, the bonding strength is 62 to 65 N. The bonding strength can be measured by the method specified in "GJB-446-1988 Adhesive 90° Peel Strength Test Method".

[0098] The aqueous polyurethane composition of the present invention has good solvent resistance after film formation and is insoluble in tetrahydrofuran.

[0099] The following describes the test method for the performance of waterborne polyurethane compositions:

[0100] Solid content: Determined by the method specified in BS EN ISO 3251-2019 Paints, varnishes and plastics - Determination of non-volatile matter content.

[0101] Viscosity: The melt viscosity at 25°C was measured using a Brookfield DV2T rotational viscometer.

[0102] Mechanical properties (tensile strength, elongation and 100% modulus): Determined by the method specified in "GB / T528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber".

[0103] Adhesive strength: Determined by the method specified in "GJB-446-1988 Adhesive 90° Peel Strength Test Method".

[0104] Solvent resistance: The waterborne polyurethane composition was cured into a film, and then cut into 50 mm × 50 mm specimens. The specimens were placed in tetrahydrofuran, and the dissolution of the specimens was observed after 6 hours.

[0105] Example 1 and Comparative Examples 1 to 3

[0106] 55 parts by weight of polycaprolactone diol (molecular weight 2000) were treated under vacuum and at a temperature of 120°C for 2 hours to obtain a dehydrated diol. The dehydrated diol was cooled to 60°C in a nitrogen atmosphere. 26 parts by weight of isophorone diisocyanate and 0.08 parts by weight of bismuth isooctanoate were added to the cooled diol and mixed evenly. The temperature of the reaction system was controlled to 85°C, and the reaction was carried out for 3 hours under stirring to obtain a prepolymer.

[0107] The prepolymer was cooled to 40° C. 6 parts by weight of dimethylolbutyric acid and 1.6 parts by weight of triethylamine were added to the cooled prepolymer, and the mixture was reacted at 60° C. for 2 hours to obtain an intermediate.

[0108] 30 parts by weight of water and sodium fatty alcohol polyoxyethylene ether carboxylate (brand name AEC-9Na, produced by Jining Fangyu Chemical Co., Ltd.) were added to the intermediate and emulsified for 5 minutes to obtain an intermediate emulsion. The intermediate emulsion was cooled to 25° C., and 75 parts by weight of water were added to the cooled intermediate emulsion for a second emulsification for 10 minutes to obtain an emulsified product.

[0109] The emulsified product, isophorone diamine and N-2-aminoethyl-3-aminopropyltriethoxysilane were reacted at 25° C. for 1 hour to obtain a waterborne polyurethane composition.

[0110] The amounts of sodium fatty alcohol polyoxyethylene ether carboxylate, isophorone diamine and N-2-aminoethyl-3-aminopropyltriethoxysilane are shown in Table 1.

[0111] The properties of the waterborne polyurethane composition are shown in Table 2.

[0112] Table 1

[0113]

[0114] Note: “—” means that this raw material is not added.

[0115] Comparative Example 4

[0116] Except that isophorone diamine was replaced by 1,4-butanediol, the rest was the same as Example 1. The properties of the waterborne polyurethane composition are shown in Table 2.

[0117] Comparative Example 5

[0118] Except that the sodium fatty alcohol polyoxyethylene ether carboxylate is replaced by hard-base phosphate ester, the rest is the same as Example 1. The properties of the waterborne polyurethane composition are shown in Table 2.

[0119] Table 2

[0120]

[0121] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A method for producing an aqueous polyurethane composition, characterized in that: The steps include: (1) treating a polymer diol as represented by formula (I) at 100 to 150° C. for 0.5 to 5 h to obtain a dehydrated diol; cooling the dehydrated diol to a temperature of ≤70° C., and then adding a diisocyanate as represented by formula (II) and a catalyst to the cooled diol to react to obtain a prepolymer; In formula (I), R5 is selected from C1-C6 alkylene groups, n represents the degree of polymerization; the molecular weight of the polymer diol is 500-4000; In formula (II), R1 to R3 are independently selected from C1 to C6 alkyl groups; R4 is selected from C1 to C6 alkylene groups; (2) reacting the prepolymer with a hydrophilic chain extender and a neutralizer to obtain an intermediate; (3) emulsifying the intermediate, 20 to 40 parts by weight of water and 0.5 to 3 parts by weight of sodium fatty alcohol polyoxyethylene ether carboxylate to obtain an intermediate emulsion; and emulsifying the intermediate emulsion with 60 to 85 parts by weight of water to obtain an emulsified product; (4) reacting the emulsified product, 3 to 8 parts by weight of a first compound represented by formula (III), and 1.5 to 4 parts by weight of a second compound represented by formula (IV) to obtain an aqueous polyurethane composition; In formula (III), R7 to R9 are independently selected from C1 to C6 alkyl groups, and R6 is selected from C1 to C6 alkylene groups; In formula (IV), R 10 ~R 12 Each of them is independently selected from a C1-C6 alkyl group, x is selected from an integer of 1-6, and y is selected from an integer of 1-6.

2. The production method according to claim 1, characterized in that The catalyst is a metal carboxylate; the metal element in the metal carboxylate is selected from one or more of bismuth and zinc; the metal carboxylate is selected from one or more of neodecanoate, isooctanoate and laurate.

3. The production method according to claim 1, characterized in that The amount of the polymer diol used is 40 to 70 parts by weight, the amount of the diisocyanate used is 15 to 35 parts by weight, and the amount of the catalyst used is 0.02 to 0.2 parts by weight.

4. The production method according to claim 1, characterized in that: In step (1), the reaction temperature is 70-100° C. and the reaction time is 1-5 h.

5. The production method according to claim 1, characterized in that: The hydrophilic chain extender is selected from one or more of dimethylol propionic acid, dimethylol butyric acid, N-methyldiethanolamine, bis-2-hydroxyethylbenzylamine, and bis-2-hydroxypropylbenzylamine; The neutralizing agent is selected from one or more of triethylamine, tripropylamine, tributylamine, dimethylcyclohexylamine, formic acid, acetic acid, hydrochloric acid, sodium hydroxide, and epichlorohydrin.

6. The production method according to claim 1, characterized in that: The amount of the hydrophilic chain extender is 2 to 9 parts by weight, and the amount of the neutralizer is 0.5 to 4 parts by weight.

7. The production method according to claim 1, characterized in that: The reaction temperature of step (2) is 45-75° C., and the reaction time is 0.5-4 h.

8. The production method according to claim 1, characterized in that: The time for the first emulsification is 1 to 8 minutes, and the time for the second emulsification is 5 to 20 minutes.

9. The production method according to claim 1, characterized in that: The polymer diol is polycaprolactone diol, the diisocyanate is isophorone diisocyanate, the first compound is isophorone diamine, and the second compound is N-2-aminoethyl-3-aminopropyltriethoxysilane.

10. An aqueous polyurethane composition, characterized in that The aqueous polyurethane composition is obtained by the production method according to any one of claims 1 to 9, and the solid content of the aqueous polyurethane composition is ≥45wt%.

Citation Information

Patent Citations

  • Solvent-free waterproof moisture-permeable waterborne polyurethane dispersion as well as preparation method and application thereof

    CN116333262A

  • Waterborne polyurethane resin dispersion and application thereof in coating

    CN116813870A

  • Preparation method of solvent-free water-based polyurethane resin

    CN104341572A

  • Water-based polyurethane emulsion with high water resistance and ethanol resistance and preparation method thereof

    CN109721707A

  • Desolvation-free water-based nonionic polyurethane and preparation method thereof

    CN112409564A