A kind of low temperature crack resistant colored emulsified asphalt and preparation method thereof
Through modified antioxidants and high-speed shearing technology, the aging problem of colored emulsified asphalt has been solved, its ductility and anti-aging properties have been improved, and the low-temperature crack resistance has been significantly improved.
Patent Information
- Application Number
- CN202410702813.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-03
AI Technical Summary
Existing colored emulsified asphalt is prone to aging under the influence of driving, rain, oxidation and ultraviolet light, has low ductility, and is difficult to maintain crack resistance.
A modified antioxidant is prepared by modifying pentaerythritol glycidyl ether on N-cyclohexyl-N'-phenyl-p-phenylenediamine, and combined with aromatic oil, petroleum resin, SBS latex, emulsifier, colorant and stabilizer. Preparation of low-temperature crack-resistant colored emulsified asphalt through high-speed shearing technology.
The ductility and anti-aging properties of colored emulsified asphalt are improved, ensuring that it still has high ductility after aging and exhibits excellent low-temperature crack resistance.
Smart Images

Figure CN118290893B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of emulsified asphalt, and in particular to a low-temperature crack-resistant colored emulsified asphalt and a preparation method thereof. Background Art
[0002] Colored emulsified asphalt is a new type of emulsified asphalt product. It not only has the performance of traditional emulsified asphalt, but also has rich colors. It can be widely used for paving colored roads, colored sidewalks in schools and parks, various colored road traffic markings, and colored spray coatings on interior and exterior walls. Because it breaks through the disadvantage of traditional emulsified asphalt that only has one black color, it has rich colors and is beautiful, so it is increasingly widely promoted and applied. However, due to the influence of driving, rain, oxidation and ultraviolet light, the colored road surface paved with conventional colored emulsified asphalt mixture is prone to aging problems.
[0003] A Chinese invention patent application with publication number CN104356588A discloses a high-concentration colored emulsified asphalt and a preparation method thereof. The colored emulsified asphalt disclosed in the Chinese invention patent application has good ductility, but the ductility is low after an aging test. Summary of the invention
[0004] In view of the deficiencies in the prior art, the object of the present invention is to provide a low-temperature crack-resistant colored emulsified asphalt and a preparation method thereof.
[0005] To achieve the above object, the present invention is implemented through the following technical solutions:
[0006] A low-temperature anti-cracking colored emulsified asphalt, comprising the following raw materials in parts by weight:
[0007] Aromatic oil: 40-45 parts, petroleum resin: 30-35 parts, SBS latex: 3-3.5 parts, emulsifier: 1.5-2.5 parts, colorant: 1-3 parts, stabilizer: 1-2 parts, modified antioxidant: 2-3 parts, deionized water: 35-40 parts;
[0008] The modified antioxidant has a structural formula as shown in formula (I):
[0009] Formula (1);
[0010] The modified antioxidant is prepared by modifying N-cyclohexyl-N'-phenyl-p-phenylenediamine with pentaerythritol glycidyl ether.
[0011] The modified antioxidant is prepared by the following method:
[0012] Add N-cyclohexyl-N'-phenyl-p-phenylenediamine, pentaerythritol glycidyl ether, and salicylic acid to the reaction bottle in sequence, stir, protect with nitrogen, heat to 160-170℃, react for 28-34h, cool to room temperature, add dichloromethane, stir and mix, then wash the separated liquid with sodium bicarbonate aqueous solution and deionized water respectively, and dry under vacuum at 70-80℃ to obtain. The reaction equation is as follows:
[0013]
[0014] The molar ratio of N-cyclohexyl-N'-phenyl-p-phenylenediamine, pentaerythritol glycidyl ether and salicylic acid is 4:(1-1.2):(0.2-0.3).
[0015] The emulsifier is one of octadecyltrimethylammonium chloride and BH-MK amide type cationic slow-cracking fast-setting asphalt emulsifier.
[0016] The stabilizer is at least one of anhydrous calcium chloride and hydroxyethyl cellulose ether.
[0017] The colorant is one of yellow iron oxide, red iron oxide and green chromium oxide.
[0018] Furthermore, a method for preparing low-temperature crack-resistant colored emulsified asphalt comprises the following steps:
[0019] S1: Heat the aromatic oil to 135-145°C, then add petroleum resin and colorant, stir and mix to obtain a mixed liquid, and keep it warm for later use;
[0020] S2: Add emulsifier, SBS latex, modified antioxidant and stabilizer to deionized water in sequence, stir and mix evenly, adjust pH to 2-3 with hydrochloric acid, and heat to 65-75°C to obtain soap solution;
[0021] S3: Add the mixed liquid of step S1 and the soap solution of step S2 into a high-speed shearing machine at the same time, and perform high-speed shearing for 30-60 minutes to obtain low-temperature crack-resistant colored emulsified asphalt.
[0022] Due to the adoption of the above technical solution, the beneficial effects of the present invention include:
[0023] (1) The present invention modifies N-cyclohexyl-N'-phenyl-p-phenylenediamine by pentaerythritol glycidyl ether to prepare a modified antioxidant suitable for SBR modified colored emulsified asphalt.
[0024] (2) The colored emulsified asphalt prepared by the present invention has a high ductility and still has a high ductility after aging, which indicates that the asphalt has excellent low-temperature crack resistance and aging resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the modified antioxidant prepared in Example 2. DETAILED DESCRIPTION
[0026] The invention will be further described below in conjunction with the embodiments, but the invention is not limited to these embodiments.
[0027] Example 1 Preparation of modified antioxidant:
[0028] 2 mol N-cyclohexyl-N'-phenyl-p-phenylenediamine, 0.5 mol pentaerythritol glycidyl ether and 0.1 mol salicylic acid were added to the reaction bottle in sequence, stirred and protected with nitrogen, heated to 170°C for reaction for 34 hours, cooled to room temperature, added with 400 g of dichloromethane and stirred to mix evenly, then washed with 8 wt% sodium bicarbonate aqueous solution twice (using 150 g of sodium bicarbonate aqueous solution each time), washed with deionized water three times (using 120 g of deionized water each time), and dried in vacuo at 75°C for 7 hours to obtain the product.
[0029] Example 2 Preparation of modified antioxidant:
[0030] 2 mol N-cyclohexyl-N'-phenyl-p-phenylenediamine, 0.55 mol pentaerythritol glycidyl ether and 0.12 mol salicylic acid were added to the reaction bottle in sequence, stirred and protected with nitrogen, heated to 165°C for reaction for 32 hours, cooled to room temperature, added with 400 g of dichloromethane and stirred to mix evenly, then washed with 8 wt% sodium bicarbonate aqueous solution twice (using 150 g of sodium bicarbonate aqueous solution each time), washed with deionized water three times (using 120 g of deionized water each time), and dried in vacuo at 70°C for 9 hours to obtain the product. Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the modified antioxidant prepared in this embodiment, the test conditions are: deuterated DMSO, 300 MHz, wherein: 3.29 ppm is the water peak, 7.79 ppm is the characteristic peak of the secondary amine (at b in the figure), 6.84-7.57 ppm is the characteristic peak of Ar-H, 5.19 ppm is the characteristic peak of the hydroxyl group (at a), 2.99 ppm is the characteristic peak at d, and the remaining peaks are the characteristic peaks of methylene and methine.
[0031] Example 3 Preparation of modified antioxidant:
[0032] 2 mol N-cyclohexyl-N'-phenyl-p-phenylenediamine, 0.6 mol pentaerythritol glycidyl ether and 0.15 mol salicylic acid were added to the reaction bottle in sequence, stirred and protected with nitrogen, heated to 160°C for reaction for 28 hours, cooled to room temperature, added with 400 g of dichloromethane and stirred to mix evenly, then washed with 8 wt% sodium bicarbonate aqueous solution twice (using 150 g of sodium bicarbonate aqueous solution each time), washed with deionized water three times (using 120 g of deionized water each time), and dried in vacuo at 80°C for 6 hours to obtain the product.
[0033] Example 4
[0034] S1: Weigh the following raw materials for use: aromatic oil: 400g, petroleum resin: 300g, SBS latex: 30g, emulsifier (octadecyltrimethylammonium chloride): 15g, colorant (iron oxide yellow): 10g, stabilizer (anhydrous calcium chloride): 10g, modified antioxidant (prepared in Example 1): 20g, deionized water: 350g;
[0035] S2: Heat the aromatic oil to 145°C, then add petroleum resin and colorant, stir and mix well to obtain a mixed liquid, and keep it warm for later use;
[0036] S3: Add emulsifier, SBS latex, modified antioxidant and stabilizer to deionized water in sequence, stir and mix evenly, adjust pH to 2 with hydrochloric acid (2 mol / L), raise the temperature to 75°C, and obtain soap solution;
[0037] S4: Add the mixed liquid of step S1 and the soap solution of step S2 into a high-speed shearing machine at the same time, and perform high-speed shearing for 30 minutes to obtain low-temperature crack-resistant colored emulsified asphalt.
[0038] Example 5
[0039] S1: Weigh the following raw materials for use: aromatic oil: 420g, petroleum resin: 325g, SBS latex: 32g, emulsifier (BH-MK amide type cationic slow cracking fast setting asphalt emulsifier): 20g, colorant (iron oxide red): 20g, stabilizer (anhydrous calcium chloride): 15g, modified antioxidant (prepared in Example 2): 25g, deionized water: 380g;
[0040] S2: Heat the aromatic oil to 140°C, then add petroleum resin and colorant, stir and mix well to obtain a mixed liquid, and keep it warm for later use;
[0041] S3: Add emulsifier, SBS latex, modified antioxidant and stabilizer to deionized water in sequence, stir and mix evenly, adjust pH to 2 with hydrochloric acid (1 mol / L), raise the temperature to 70°C, and obtain soap solution;
[0042] S4: Add the mixed liquid of step S1 and the soap solution of step S2 into a high-speed shearing machine at the same time, and perform high-speed shearing for 45 minutes to obtain low-temperature crack-resistant colored emulsified asphalt.
[0043] Example 6
[0044] S1: Weigh the following raw materials for use: aromatic oil: 450g, petroleum resin: 350g, SBS latex: 35g, emulsifier (BH-MK amide type cationic slow cracking and fast setting asphalt emulsifier): 25g, colorant (chromium oxide green): 30g, stabilizer (hydroxyethyl cellulose ether): 10g, stabilizer (anhydrous calcium chloride): 10g, modified antioxidant (prepared in Example 3): 30g, deionized water: 400g;
[0045] S2: Heat the aromatic oil to 135°C, then add petroleum resin and colorant, stir and mix well to obtain a mixed liquid, and keep it warm for later use;
[0046] S3: Add emulsifier, SBS latex, modified antioxidant and stabilizer to deionized water in sequence, stir and mix evenly, adjust pH to 3 with hydrochloric acid (0.8 mol / L), raise the temperature to 65°C, and obtain soap solution;
[0047] S4: Add the mixed liquid of step S1 and the soap solution of step S2 into a high-speed shearing machine at the same time, and perform high-speed shearing for 60 minutes to obtain low-temperature crack-resistant colored emulsified asphalt.
[0048] Comparative Example 1
[0049] The raw material composition and preparation method of the colored emulsified asphalt are basically the same as those in Example 5, except that no modified antioxidant (prepared in Example 2) is added.
[0050] Comparative Example 2
[0051] The raw material composition and preparation method of the colored emulsified asphalt are basically the same as those in Example 5, except that the modified antioxidant (prepared in Example 2) is replaced by an equal mass of N-cyclohexyl-N'-phenyl-p-phenylenediamine.
[0052] Comparative Example 3
[0053] The raw material composition and preparation method of the colored emulsified asphalt are basically the same as those in Example 5, except that the modified antioxidant (prepared in Example 2) is replaced with an equal mass of phenyl glycidyl ether-modified N-cyclohexyl-N'-phenyl-p-phenylenediamine. The preparation method of phenyl glycidyl ether-modified N-cyclohexyl-N'-phenyl-p-phenylenediamine is as follows:
[0054] 2 mol N-cyclohexyl-N'-phenyl-p-phenylenediamine, 2.2 mol phenyl glycidyl ether and 0.12 mol salicylic acid were added to the reaction bottle in sequence, stirred and protected with nitrogen, heated to 165°C for reaction for 32 hours, cooled to room temperature, added with 400 g of dichloromethane and stirred to mix evenly, then washed with 8 wt% sodium bicarbonate aqueous solution twice (using 150 g of sodium bicarbonate aqueous solution each time), washed with deionized water three times (using 120 g of deionized water each time), and dried in vacuo at 70°C for 9 hours to obtain the product.
[0055] Comparative Example 4
[0056] The raw material composition and preparation method of the colored emulsified asphalt are basically the same as those in Example 5, except that the modified antioxidant (prepared in Example 2) is replaced with an equal mass of glycidyl ether (CAS No.: 13236-02-7) modified N-cyclohexyl-N'-phenyl-p-phenylenediamine. The preparation method of glycidyl ether modified N-cyclohexyl-N'-phenyl-p-phenylenediamine is as follows:
[0057] 2 mol N-cyclohexyl-N'-phenyl-p-phenylenediamine, 0.7 mol glycidyl ether and 0.12 mol salicylic acid were added to the reaction bottle in sequence, stirred and protected with nitrogen, heated to 165°C for reaction for 32 hours, cooled to room temperature, added with 400 g of dichloromethane and stirred to mix evenly, then washed with 8 wt% sodium bicarbonate aqueous solution twice (using 150 g of sodium bicarbonate aqueous solution each time), washed with deionized water three times (using 120 g of deionized water each time), and dried in vacuo at 70°C for 9 hours to obtain the product.
[0058] Comparative Example 5
[0059] The raw material composition and preparation method of the colored emulsified asphalt are basically the same as those of Example 5, except that the modified antioxidant (prepared in Example 2) is replaced with an equal mass of N-isopropyl-N'-phenyl-p-phenylenediamine modified with pentaerythritol glycidyl ether. The preparation method of N-isopropyl-N'-phenyl-p-phenylenediamine modified with pentaerythritol glycidyl ether is as follows:
[0060] 2 mol N-isopropyl-N'-phenyl-p-phenylenediamine, 0.55 mol pentaerythritol glycidyl ether and 0.12 mol salicylic acid were added to the reaction bottle in sequence, stirred and protected with nitrogen, heated to 165°C for reaction for 32 hours, cooled to room temperature, added with 400 g of dichloromethane and stirred to mix evenly, then washed with 8 wt% sodium bicarbonate aqueous solution twice (using 150 g of sodium bicarbonate aqueous solution each time), washed with deionized water three times (using 120 g of deionized water each time), and dried in vacuo at 70°C for 9 hours to obtain the product.
[0061] Comparative Example 6
[0062] The colored asphalt is prepared using the raw materials and preparation method of Example 1 in publication number CN106832846A.
[0063] Comparative Example 7
[0064] The raw material composition and preparation method of the colored emulsified asphalt are basically the same as those in Example 5, except that the modified antioxidant (prepared in Example 2) is replaced by 18 g of N-cyclohexyl-N'-phenyl-p-phenylenediamine and 8 g of pentaerythritol glycidyl ether.
[0065] The aromatic oil used in the examples and comparative examples of the present application is a vacuum four-line furfural refined extraction oil in the petroleum refining process, purchased from Shanghai Gaoqiao Petrochemical Company of Sinopec, with an open flash point of 232°C and a kinematic viscosity of 29 mm at 100°C. 2 / s, aromatic content 82wt%; petroleum resin is C9 petroleum resin, purchased from Shandong Qilong Chemical Co., Ltd., brand R110, softening point 110℃; BH-MK amide type cationic slow cracking and fast setting asphalt emulsifier was purchased from Shandong Banghua Oil Chemical Co., Ltd.; SBS latex was purchased from Shandong Dashan Road and Bridge Engineering Co., Ltd., solid content 42.5wt%, pH=5.6, average particle size 1.96μm.
[0066] The high-speed shearing machine in the embodiment of the present application and the comparative example maintained a shearing temperature of 140±5° C. and a shearing speed of 6500 rpm during shearing.
[0067] The colored emulsified asphalt prepared in Examples 4-6 of the present application and Comparative Examples 1-7 were tested for penetration (T 0604-2011), softening point (T 0606-2011), ductility (T 0605-2011), and aging performance (T0610-2011) according to the requirements of JTG E20-2011 standard. The test results are shown in Table 1.
[0068] Table 1
[0069]
[0070] It can be seen from the data in Table 1 that the colored emulsified asphalt prepared in Examples 4-6 of the present application has an elongation of >41 cm at 5°C, a needle penetration of less than 66 (100 g, 5 s, 25°C / 0.1 mm), and an elongation of >30 cm at 5°C after the aging test, and has excellent low-temperature crack resistance and anti-aging properties.
[0071] Comparative Example 1 is a comparative example without adding antioxidant, and its elongation at 5°C after aging is only 22.3 cm.
[0072] The antioxidants added in Comparative Examples 2, 3, 4 and 5 are respectively N-cyclohexyl-N'-phenyl-p-phenylenediamine, phenyl glycidyl ether-modified N-cyclohexyl-N'-phenyl-p-phenylenediamine, glycidyl ether-modified N-cyclohexyl-N'-phenyl-p-phenylenediamine and pentaerythritol glycidyl ether-modified N-isopropyl-N'-phenyl-p-phenylenediamine. It can be seen from the data in Table 1 that the elongation at 5°C after aging is less than 27.1 cm.
[0073] Comparative Example 6 is a colored asphalt prepared using the raw materials and preparation method of Example 1 of the Chinese invention patent with publication number CN106832846A. Its elongation at 5°C after aging is only 23.6 cm.
[0074] Comparative Example 7 is a comparative example in which N-cyclohexyl-N'-phenyl-p-phenylenediamine and pentaerythritol glycidyl ether are added as antioxidants. The elongation at 5°C after aging is only 24.5 cm.
[0075] The reason why N-cyclohexyl-N'-phenyl-p-phenylenediamine has poor anti-aging performance is that its molecular weight is relatively small, it is easy to volatilize, and it is not resistant to migration and extraction. The present application modifies N-cyclohexyl-N'-phenyl-p-phenylenediamine by pentaerythritol glycidyl ether, which, on the one hand, increases the molecular weight of the anti-aging and improves the migration and extraction resistance of the anti-aging; on the other hand, the modified anti-aging provides more secondary amine and hydroxyl groups for capturing free radicals.
[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. However, any equivalent changes, modifications and evolutions made by ordinary technicians in the field without departing from the scope of the technical solution of the present invention by using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.
Claims
1. An emulsified asphalt, characterized in that: The invention comprises the following raw materials in parts by weight: Aromatic oil: 40-45 parts, petroleum resin: 30-35 parts, SBS latex: 3-3.5 parts, emulsifier: 1.5-2.5 parts, colorant: 1-3 parts, stabilizer: 1-2 parts, modified antioxidant: 2-3 parts, deionized water: 35-40 parts; The modified antioxidant is prepared by modifying N-cyclohexyl-N'-phenyl-p-phenylenediamine with pentaerythritol glycidyl ether, and the preparation method is as follows: Add N-cyclohexyl-N'-phenyl-p-phenylenediamine, pentaerythritol glycidyl ether and salicylic acid to a reaction flask in sequence, stir, protect with nitrogen, heat to 160-170°C and react for 28-34h, cool to room temperature, add dichloromethane and stir to mix, then wash the separated liquids with sodium bicarbonate aqueous solution and deionized water respectively, and dry in vacuum at 70-80°C to obtain; The molar ratio of N-cyclohexyl-N'-phenyl-p-phenylenediamine, pentaerythritol glycidyl ether and salicylic acid is 4:(1-1.2):(0.2-0.3).
2. An emulsified asphalt according to claim 1, characterized in that: The emulsifier is one of octadecyltrimethylammonium chloride and BH-MK amide type cationic slow-cracking fast-setting asphalt emulsifier.
3. An emulsified asphalt according to claim 1, characterized in that: The stabilizer is at least one of anhydrous calcium chloride and hydroxyethyl cellulose ether.
4. The emulsified asphalt according to claim 1, characterized in that: The colorant is one of yellow iron oxide, red iron oxide and green chromium oxide.
5. A method for preparing emulsified asphalt according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1: Heat the aromatic oil to 135-145°C, then add petroleum resin and colorant, stir and mix to obtain a mixed liquid, and keep it warm for later use; S2: Add emulsifier, SBS latex, modified antioxidant and stabilizer to deionized water in sequence, stir and mix evenly, adjust pH to 2-3 with hydrochloric acid, and heat to 65-75°C to obtain soap solution; S3: Add the mixed liquid of step S1 and the soap solution of step S2 into a high-speed shearing machine at the same time, and perform high-speed shearing for 30-60 minutes to obtain low-temperature crack-resistant colored emulsified asphalt.