Composite electrode and preparation method thereof and solar cell

By using alternating stacked structures and protective layers in the preparation of composite electrodes, the problems of low battery conversion efficiency and easy oxidation of silver-clad copper paste are solved, and a composite electrode with low cost, high efficiency and stability is realized, replacing the traditional wire mesh Printing process.

CN118315452BActive Publication Date: 2024-11-08SHENZHEN APG MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410460250.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-17
Publication Date
2024-11-08
Estimated Expiration
2044-04-17

AI Technical Summary

Technical Problem

The existing methods for preparing composite electrodes have problems such as low cell conversion efficiency and easy oxidation of silver-clad copper paste, and traditional solutions such as the addition of stabilizers or sintering processes increase costs and time.

Method used

The metal gate wire groove is prepared on the substrate, the composite silver paste is coated to form a first protective layer, and the copper paste and the composite silver paste are stacked alternately to form an alternately stacked composite core, and then bonded to the solar cell. A second protective layer is formed, the substrate is removed, and a composite electrode is produced.

Benefits of technology

It improves the photoelectric conversion efficiency of the battery, reduces the amount and cost of silver paste, prevents oxidation of the copper layer, extends the battery life, and reduces contact resistance, replacing the traditional screen printing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118315452B_ABST
    Figure CN118315452B_ABST
Patent Text Reader

Abstract

The present invention provides a composite electrode and a preparation method thereof and a solar cell, belonging to the technical field of solar electrode. The preparation method includes: providing a substrate, preparing a groove of a metal grid line on the substrate; coating a composite silver paste on the groove wall of the groove, performing a first curing treatment, and forming a first protective layer on the inner surface of the groove; coating the first protective layer of the groove in the order of alternating copper paste and composite silver paste, and performing a pre-curing treatment after coating the copper paste or the composite silver paste, until the copper paste and the composite silver paste fill the groove, and then performing a second curing treatment to obtain a composite core with copper layers and composite silver layers alternately stacked; coating the composite silver paste on the surface of the composite core away from the substrate, and then performing a bonding treatment with a solar cell to be metallized, and then performing a third curing treatment to form a second protective layer, and removing the substrate to obtain a composite electrode. The composite electrode prepared by the present invention has the characteristics of low cost, high conversion efficiency and good oxidation resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solar electrode, and in particular relates to a composite electrode and a preparation method thereof and a solar cell. Background Art

[0002] In recent years, silver-coated copper paste has been widely used as an electrode material to reduce the cost of solar cell metallization. However, silver-coated copper paste is prone to oxidation during long-term use, resulting in a decrease in cell performance and limiting the life and conversion efficiency of solar cells.

[0003] Prior art 1:

[0004] The existing solution is to inhibit the oxidation of silver-coated copper paste by adding stabilizers. However, this method has certain limitations. The stabilizer will have a negative impact on the performance of the battery, reduce the conversion efficiency of solar energy, and shorten the life of the solar cell.

[0005] Prior art 2:

[0006] The existing solution can also use the method of sintering in an atmosphere furnace to inhibit the oxidation of the silver-clad copper paste. However, sintering in an atmosphere furnace will greatly increase the process cost and time, because adding the sintering process in an atmosphere furnace means adding a plant, purchasing equipment, extending the process section, debugging the process, controlling the sintering yield, etc., and the economic benefits are poor.

[0007] Therefore, it is necessary to develop a preparation method for a composite electrode that can reduce costs and is not easily oxidized, while not affecting or even improving battery conversion efficiency. Summary of the invention

[0008] The purpose of the present invention is to provide a composite electrode and a preparation method thereof, aiming to solve the problems of low battery conversion efficiency and easy oxidation of silver-coated copper paste in the existing composite electrode preparation method. To achieve the above purpose, the present application adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing a composite electrode, comprising the following steps:

[0010] Providing a substrate, and preparing a groove for a metal gate line on the substrate;

[0011] Applying the composite silver paste on the groove wall of the groove, performing a first curing treatment, and forming a first protective layer on the inner surface of the groove;

[0012] Coating the copper paste and the composite silver paste in the first protective layer of the groove in an alternating order, and performing a pre-curing treatment after coating the copper paste or the composite silver paste until the copper paste and the composite silver paste fill the groove, and then performing a second curing treatment to obtain a composite core with copper layers and composite silver layers alternately stacked;

[0013] The composite silver paste is coated on the surface of the composite core away from the substrate, and then the composite core is bonded to the solar cell sheet to be metallized, and then a third curing treatment is performed to form a second protective layer, and the substrate is removed to obtain a composite electrode.

[0014] In a second aspect, the present invention provides a composite electrode, which is prepared by the preparation method provided in the present application.

[0015] In a third aspect, the present invention provides a solar cell comprising the composite electrode provided in the present application.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] The preparation method of the composite electrode provided by the first aspect of the present invention is to first prepare a groove of the metal grid line on the substrate as a mold for preparing the composite electrode, and then form a first protective layer on the groove wall of the groove with a composite silver paste, and then apply the copper paste and the composite silver paste in the first protective layer to form a composite core with copper layers and composite silver layers alternately stacked, and finally apply the composite silver paste on the surface of the composite core, and solidify it after being bonded to the solar cell to be metallized to form a second protective layer, and remove the substrate to obtain the composite electrode. Therefore, on the one hand, the molding method using the embossed groove as the mold has a high molding degree and the obtained solar electrode has a larger aspect ratio, which can reduce the loss of photogenerated carriers, reduce the blocking of sunlight, improve the photoelectric conversion efficiency, and reduce the amount of silver paste, thereby reducing the cost. On the other hand, the first protective layer and the second protective layer in the composite electrode of the present invention play a role in completely isolating the air, preventing the copper layer in the composite core from contacting the air, and protecting the copper layer from oxidation. Moreover, the composite core is an alternating laminated structure of composite silver layer and copper layer. The multi-layer composite silver layer in the composite core plays a role in strengthening the protection of the copper layer. Even if the first protective layer is damaged, the multi-layer composite silver layer can still protect the copper layer in the composite core from being oxidized, thereby maintaining the stability of the solar cell. In addition, by using composite silver paste to form a multi-element alloy at the interface between the layers, the contact resistance at the interface between the first protective layer, the composite silver layer, the copper layer, and the second protective layer can be greatly reduced, thereby further improving the photoelectric conversion efficiency of the solar cell. Therefore, the preparation method of the present invention is expected to replace the traditional screen printing process.

[0018] The composite electrode provided in the second aspect of the present invention has the advantages of low cost, good oxidation resistance and high conversion efficiency, because it is prepared by the composite electrode preparation method provided by the present invention.

[0019] The solar cell provided in the third aspect of the present invention has the advantages of low cost, high conversion efficiency and good stability because it includes the composite electrode provided in the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0021] Figure 1 This is a schematic structural diagram of the composite electrode provided by the present invention. DETAILED DESCRIPTION

[0022] The embodiments of the present application will be described in detail below in conjunction with specific examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present application and should not be considered to limit the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the materials or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially.

[0023] In view of the above technical problems, this application proposes an innovative solution, which aims to solve the problems of low battery conversion efficiency and easy oxidation of silver-coated copper paste in the existing composite electrode preparation method, while not affecting the performance of solar cells. This application can not only be applied to the production process of solar cells, but also has broad application prospects and can be extended to the preparation of electronic devices in other fields, providing new ideas and methods for improving the stability and performance of electronic devices.

[0024] Combination Figure 1 The first aspect of the embodiment of the present invention provides a method for preparing a composite electrode, comprising the following steps:

[0025] S01: providing a substrate, and preparing grooves for metal gate lines on the substrate;

[0026] S02: coating the composite silver paste on the groove wall of the groove, performing a first curing treatment, and forming a first protective layer on the inner surface of the groove;

[0027] S03: Coating the copper paste and the composite silver paste in the first protective layer of the groove in an alternating order, and performing a pre-curing treatment after coating the copper paste or the composite silver paste until the copper paste and the composite silver paste fill the groove, and then performing a second curing treatment to obtain a composite core with copper layers and composite silver layers alternately stacked;

[0028] S04: coating the composite silver paste on the surface of the composite core facing away from the substrate, and then laminating it with the solar cell sheet to be metallized, and then performing a third curing treatment to form a second protective layer, removing the substrate, and obtaining a composite electrode.

[0029] The preparation method of the composite electrode provided by the embodiment of the present invention is to first prepare a groove of the metal grid line on the substrate as a mold for preparing the composite electrode, and then form a first protective layer on the groove wall of the groove with a composite silver paste, and then apply the copper paste and the composite silver paste in the first protective layer to form a composite core with copper layers and composite silver layers alternately stacked, and finally apply the composite silver paste on the surface of the composite core, and solidify it after being bonded to the solar cell to be metallized to form a second protective layer, and remove the substrate to obtain the composite electrode. Therefore, on the one hand, the molding method using the embossed groove as the mold has a high molding degree and the obtained solar electrode has a larger aspect ratio, which can reduce the loss of photogenerated carriers, reduce the blocking of sunlight, improve the photoelectric conversion efficiency, and reduce the amount of silver paste used, thereby reducing the cost. On the other hand, the first protective layer and the second protective layer in the composite electrode of the present invention play a role in isolating the air, preventing the copper layer in the composite core from contacting the air, and protecting the copper layer from oxidation. Moreover, the composite core is an alternating laminated structure of composite silver layer and copper layer. The multi-layer composite silver layer in the composite core plays a role in strengthening the protection of the copper layer. Even if the first protective layer is damaged, the composite silver layer can still protect the copper layer in the composite core from oxidation, thereby maintaining the stability of the solar cell. In addition, by using composite silver paste to form a multi-element alloy at the interface between the layers, the contact resistance at the interface between the first protective layer, the composite silver layer, the copper layer, and the second protective layer can be greatly reduced, thereby further improving the photoelectric conversion efficiency of the solar cell. Therefore, the preparation method of the present invention is expected to replace the traditional screen printing process.

[0030] In step S01 , the substrate may be a transparent substrate.

[0031] In some embodiments, the step of preparing the groove of the metal grid line on the substrate includes: coating a photosensitive adhesive or a thermoplastic adhesive on the substrate, and then stamping out the groove of the metal grid line, wherein the photosensitive adhesive includes a photoresist or a UV adhesive.

[0032] In some embodiments, the groove has a width of 10-40 μm and a depth of 20-60 μm.

[0033] In some embodiments, before the step of coating the composite silver paste on the groove wall of the groove, the step further includes performing a surface oleophobic treatment on the groove wall of the groove to reduce the difficulty of subsequent groove stripping or to avoid direct contact between the silver paste and the groove. The surface oleophobic treatment may be plasma treatment, or coating a release agent on the groove wall of the groove.

[0034] In step S02, the composite silver paste includes the following components in parts by weight: 60-80 parts of silver powder, 0.1-5 parts of tin-nickel alloy powder, 10-40 parts of organic carrier, and 0.1-1 parts of antioxidant. Since the metal activity of tin and nickel is stronger than that of silver and copper, when the composite silver paste with tin-nickel alloy powder added is cured, tin and nickel easily form multi-element alloys such as silver-tin alloy and copper-nickel alloy at the interface of silver and copper, which can enhance the interface contact between the first protective layer and the composite core, thereby greatly reducing the contact resistance at the interlayer interface and improving the photoelectric conversion efficiency of the solar cell. In addition, since the solar spectrum absorption rate of the tin-nickel alloy powder is high, the first protective layer formed after the composite silver paste with tin-nickel alloy powder added is cured can increase the absorption of the solar spectrum by the solar cell, thereby further improving the photoelectric conversion efficiency of the solar cell.

[0035] In some embodiments, the mass ratio of tin to nickel in the tin-nickel alloy powder is 3 / (1-2).

[0036] In some embodiments, the particle size of the tin-nickel alloy powder is 1-6 μm. The particle size of the tin-nickel alloy powder in this range matches the particle size of the silver powder, which is conducive to uniform mixing.

[0037] In some embodiments, the silver powder is composed of spherical silver powder and flake silver powder in a mass ratio of (0.5-1.5) / 3.

[0038] In some embodiments, the organic carrier may be selected from at least one of epoxy resin, phenolic resin, ethyl cellulose, and acrylic resin.

[0039] In some embodiments, the antioxidant may be selected from at least one of polyvinyl pyrrolidone, 2,6-di-tert-butyl-p-cresol, and ascorbic acid. These antioxidants can effectively prevent the metal in the composite silver paste from being oxidized.

[0040] In some embodiments, the viscosity of the composite silver paste is 120,000-230,000 cps.

[0041] In some embodiments, the first curing treatment conditions include: 100-2500 MJ / cm 2 UV light irradiation for 5 to 60 seconds.

[0042] In some embodiments, the thickness of the first protective layer is 0.5 to 5 μm. If the first protective layer is too thin, it is difficult to completely cover the composite core, and the protection effect of the copper layer in the composite core is not good; if the first protective layer is too thick, it is not conducive to reducing costs; therefore, the thickness range of the first protective layer in this embodiment can completely and continuously cover the composite core while ensuring low costs, isolate the copper layer in the composite core from contact with the air, prevent oxidation of the copper layer, and the first protective layer is not easy to be damaged, which plays a good protective role on the copper layer, so that the solar cell has better stability.

[0043] In step S03, the copper paste and the composite silver paste are formed into a composite core with copper layers and composite silver layers alternately stacked. On the one hand, since the metal activity of tin and nickel is stronger than that of silver and copper, when the composite silver paste with tin-nickel alloy powder added is solidified, tin and nickel are easy to form multi-element alloys such as silver-tin alloy and copper-nickel alloy at the interface of silver and copper, which can enhance the contact between the composite silver layer and the copper layer, thereby greatly reducing the contact resistance at the interlayer interface and improving the photoelectric conversion efficiency of the solar cell; on the other hand, the multi-layer composite silver layer in the composite core plays a role in strengthening the protection of the copper layer. Even if the first protective layer is damaged, the composite silver layer can still protect the copper layer in the composite core from being oxidized, thereby maintaining the stability of the solar cell. In addition, since the thermal emissivity of the tin-nickel alloy powder is low, the composite core formed after the composite silver paste with tin-nickel alloy powder added is solidified can reduce the energy loss caused by the heating of the electrode, thereby further improving the photoelectric conversion efficiency of the solar cell.

[0044] In some embodiments, the steps of preparing a composite core in which copper layers and composite silver layers are alternately stacked may include: coating copper paste on the inner surface of the first protective layer of the groove, and then pre-curing to form a copper paste layer; coating the composite silver paste on the inner surface of the copper paste layer, and then pre-curing to form a composite silver paste layer; coating the copper paste on the inner surface of the composite silver paste layer of the groove, and then pre-curing to form a copper paste layer; coating the composite silver paste on the inner surface of the copper paste layer, and then pre-curing to form a composite silver paste layer; ... and so on, until the copper paste and the composite silver paste fill the groove, and a second curing treatment is performed to obtain a composite core in which copper layers and composite silver layers are alternately stacked.

[0045] In some embodiments, the copper paste includes any one of sintered copper paste, thermally cured copper paste or ultraviolet light cured copper paste. These copper pastes can be directly purchased from the market for use.

[0046] In some embodiments, the pre-curing conditions may include: heating at 50-100° C. for 5-10 min, or at 50-500 MJ / cm 2 Irradiate under UV light for 5 to 10 seconds.

[0047] In some embodiments, the second curing treatment conditions include: 100-2500 MJ / cm 2 Irradiate with UV light for 10 to 60 minutes.

[0048] In step S04, the second protective layer can effectively prevent oxygen in the air from entering the composite core from the TCO layer or the anti-reflection layer of the solar cell, and can further enhance the protective effect on the copper layer in the composite core.

[0049] In some embodiments, the conditions of the third curing treatment include: 50-3000 MJ / cm2 UV light irradiation for 5 to 60 seconds.

[0050] In some embodiments, the thickness of the second protective layer is 0.5 to 5 μm. If the second protective layer is too thin, oxygen in the air can easily enter the composite core from the TCO layer or the anti-reflection layer of the solar cell, and the protective effect on the copper layer in the composite core is poor; if the second protective layer is too thick, it is not conducive to reducing costs; therefore, the thickness range of the second protective layer in this embodiment can completely and continuously cover the composite core while ensuring low costs, isolating the copper layer in the composite core from contact with the air, and preventing oxidation of the copper layer.

[0051] In some embodiments, the solar cell may be a conventional back cell (PERC), a heterojunction solar cell (HJT), or a tunneling oxide passivation contact cell (TOPCon). If the solar cell is a heterojunction solar cell, the TCO layer of the solar cell to be metallized is laminated with the composite silver paste coated on the surface of the composite core to form a second protective layer. If the solar cell is a conventional back cell or a tunneling oxide passivation contact cell, the anti-reflection layer of the solar cell to be metallized is laminated with the composite silver paste coated on the surface of the composite core to form a second protective layer.

[0052] A second aspect of an embodiment of the present invention provides a composite electrode, which is prepared by the preparation method provided in this application.

[0053] The composite electrode provided in the embodiment of the present invention has the advantages of low cost, good oxidation resistance and high conversion efficiency, because it is prepared by the composite electrode preparation method provided by the present invention.

[0054] A third aspect of an embodiment of the present invention provides a solar cell, which includes the composite electrode provided in this application.

[0055] The solar cell provided by the embodiment of the present invention has the advantages of low cost, high conversion efficiency and good stability because it includes the composite electrode provided by the present application.

[0056] The following describes the invention in conjunction with specific embodiments.

[0057] Example 1

[0058] This embodiment provides a method for preparing a composite electrode, comprising the following steps:

[0059] (1) coating a photoresist layer on a transparent substrate, and using a preset relief mold to print out grooves for metal grid lines of solar cells, wherein the grooves for the metal grid lines have a width of 20 μm and a depth of 30 μm;

[0060] (2) Apply a composite silver paste with a viscosity of 200,000 cps on the groove wall at 1000 MJ / cm 2 The first protective layer was irradiated with UV light for 30 seconds to obtain a first protective layer with a thickness of 2.5 μm;

[0061] (3) Coat the first protective layer of the groove with commercially available copper paste at 200 MJ / cm 2 The copper paste layer was formed by irradiating the copper paste layer with UV light for 5 seconds. Then, the composite silver paste was coated in the copper paste layer and the copper paste layer was exposed to UV light at 200 MJ / cm 2 The composite silver paste layer was formed by irradiating the composite silver paste layer with UV light of 200 MJ / cm 2 The copper paste layer was formed by irradiating the copper paste layer with UV light for 5 seconds. Then, the composite silver paste was coated on the copper paste layer. 2 The composite silver paste layer was formed by irradiating the groove with the UV light for 5s. Finally, the copper paste was filled into the groove and the 2 The composite core is irradiated with UV light for 30 min to obtain a composite core having copper layers and composite silver layers alternately stacked;

[0062] (4) The composite silver paste is coated on the surface of the composite core facing away from the substrate, and then the composite silver paste is laminated with the anti-reflection layer of the solar cell to be metallized and a certain pressure is applied to ensure that the composite silver paste and the anti-reflection layer are in full contact. 2 The electrode was irradiated with UV light for 30 seconds to form a second protective layer with a thickness of 2.5 μm, and the substrate was removed to obtain a composite electrode;

[0063] Among them, the composite silver paste is composed of 72 parts of silver powder, 2.5 parts of tin-nickel alloy powder, 25 parts of epoxy resin (organic carrier) and 0.5 parts of polyvinyl pyrrolidone (antioxidant); the particle size of the tin-nickel alloy powder is 4μm, and the mass ratio of tin to nickel is 3 / 2; the silver powder is composed of spherical silver powder (average particle size is 0.4μm) and flaky silver powder (average particle size is 5μm) with a mass ratio of 1 / 3.

[0064] Example 2

[0065] This embodiment provides a method for preparing a composite electrode, which differs from Embodiment 1 in that the composite silver paste consists of 74.4 parts of silver powder, 0.1 parts of tin-nickel alloy powder, 25 parts of epoxy resin and 0.5 parts of polyvinyl pyrrolidone.

[0066] Example 3

[0067] This embodiment provides a method for preparing a composite electrode, which differs from Embodiment 1 in that the composite silver paste consists of 69.5 parts of silver powder, 5 parts of tin-nickel alloy powder, 25 parts of epoxy resin and 0.5 parts of polyvinyl pyrrolidone.

[0068] Example 4

[0069] This embodiment provides a method for preparing a composite electrode, which differs from Embodiment 1 in that the composite silver paste consists of 60 parts of silver powder, 2.5 parts of tin-nickel alloy powder, 37 parts of epoxy resin and 0.5 parts of polyvinyl pyrrolidone.

[0070] Example 5

[0071] This embodiment provides a method for preparing a composite electrode, which differs from Embodiment 1 in that the composite silver paste is composed of 80 parts of silver powder, 2.5 parts of tin-nickel alloy powder, 17 parts of epoxy resin and 0.5 parts of polyvinyl pyrrolidone, wherein the silver powder is 60 parts.

[0072] Example 6

[0073] This embodiment provides a method for preparing a composite electrode, which differs from Embodiment 1 in that the thickness of the first protective layer is 5 μm, and the thickness of the second protective layer is 5 μm.

[0074] Example 7

[0075] This embodiment provides a method for preparing a composite electrode, which differs from Embodiment 1 in that the thickness of the first protective layer is 0.5 μm, and the thickness of the second protective layer is 0.5 μm.

[0076] Example 8

[0077] This embodiment provides a method for preparing a composite electrode, which differs from Embodiment 1 in that the composite silver paste consists of 64.5 parts of silver powder, 10 parts of tin-nickel alloy powder, 25 parts of epoxy resin and 0.5 parts of polyvinyl pyrrolidone.

[0078] Example 9

[0079] This embodiment provides a method for preparing a composite electrode, which differs from Embodiment 1 in that the composite silver paste consists of 74.49 parts of silver powder, 0.01 parts of tin-nickel alloy powder, 25 parts of epoxy resin and 0.5 parts of polyvinyl pyrrolidone.

[0080] Comparative Example 1

[0081] This comparative example provides an electrode, which is prepared by coating DD-1760 series silver paste on the anti-reflection layer of a solar cell by screen printing and then sintering.

[0082] Comparative Example 2

[0083] This comparative example provides a composite electrode, which is prepared by coating a commercially available silver-coated copper paste on an anti-reflection layer of a solar cell by screen printing and then sintering the paste.

[0084] Comparative Example 3

[0085] This comparative example provides a method for preparing a composite electrode, comprising the following steps:

[0086] (1) coating a photoresist layer on a transparent substrate, and using a preset relief mold to print out grooves for metal grid lines of solar cells, wherein the grooves for the metal grid lines have a width of 20 μm and a depth of 30 μm;

[0087] (2) Apply a composite silver paste with a viscosity of 200,000 cps on the groove wall at 1000 MJ / cm 2 The first protective layer was irradiated with UV light for 30 seconds to obtain a first protective layer with a thickness of 2.5 μm;

[0088] (3) Fill the groove with commercially available copper paste at 2000 MJ / cm 2 Irradiate under UV light for 30 min to obtain a copper layer;

[0089] (4) The composite silver paste is coated on the surface of the copper layer facing away from the substrate, and then the composite silver paste is laminated with the anti-reflection layer of the solar cell to be metallized and a certain pressure is applied to ensure that the composite silver paste and the anti-reflection layer are in full contact. 2 The electrode was irradiated with UV light for 30 seconds to form a second protective layer with a thickness of 2.5 μm, and the substrate was removed to obtain a composite electrode;

[0090] Among them, the composite silver paste is composed of 72 parts of silver powder, 2.5 parts of tin-nickel alloy powder, 25 parts of epoxy resin and 0.5 parts of polyvinyl pyrrolidone; the particle size of the tin-nickel alloy powder is 4μm, and the mass ratio of tin to nickel is 3 / 2; the silver powder is composed of spherical silver powder (average particle size is 0.4μm) and flaky silver powder (average particle size is 5μm) with a mass ratio of 1 / 3; the thickness of the first protective layer is 3μm.

[0091] Comparative Example 4

[0092] This comparative example provides a method for preparing a composite electrode. The difference between this comparative example and Example 1 is that the second protective layer is not prepared in this comparative example, that is, the prepared composite electrode does not contain the second protective layer.

[0093] Comparative Example 5

[0094] This comparative example provides a method for preparing a composite electrode. The difference between this comparative example and Example 1 is that the composite silver paste in steps (2), (3) and (4) is replaced with commercially available silver paste.

[0095] Related performance test analysis:

[0096] 1. The composite electrodes prepared in Examples 1 to 9 and Comparative Examples 1 to 5 were assembled into solar cells to test line height, line width, aspect ratio and conversion efficiency (the conversion efficiency was based on Comparative Example 1, and the test value was the value increased or decreased relative to the photoelectric conversion efficiency of Comparative Example 1). The test results are shown in Table 1:

[0097] Table 1

[0098]

[0099] It can be seen from Table 1 that the aspect ratio and conversion efficiency of the composite electrodes prepared in Examples 1 to 9 are significantly higher than the aspect ratio and conversion efficiency of the electrodes prepared by screen printing in Comparative Examples 1 to 2, indicating that the molding method using the embossed groove as a mold in the embodiments of the present invention has a high degree of molding and the prepared composite electrode has a larger aspect ratio. Therefore, it can reduce the loss of photogenerated carriers, reduce the shielding of sunlight, and improve the conversion efficiency.

[0100] The composite electrodes prepared in Examples 1 to 9 did not fall off or oxidize, while Comparative Example 4 oxidized, indicating that the composite electrode of the present invention can further strengthen the protection of the copper layer in the composite core through the second protective layer, and can prevent oxygen in the air from entering the composite core from the TCO layer or the anti-reflection layer of the solar cell, thereby effectively avoiding oxidation of the copper layer.

[0101] The battery conversion efficiency of the composite electrodes prepared in Examples 1 to 9 is significantly higher than that of the composite electrodes prepared in Comparative Examples 3 and 5, indicating that when the composite silver paste of the present invention is cured, the tin and nickel in the tin-nickel alloy powder form a multi-element alloy at the interface of silver and copper, which can greatly reduce the contact resistance at the interlayer interface, thereby improving the photoelectric conversion efficiency of the solar cell.

[0102] In summary, the composite electrode prepared by the present invention has the advantages of low cost, high conversion efficiency and good oxidation resistance, and can be used to replace the traditional screen printing process.

[0103] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a composite electrode, characterized in that: The steps include: Providing a substrate, and preparing a groove for a metal gate line on the substrate; Applying the composite silver paste on the groove wall of the groove, performing a first curing treatment, and forming a first protective layer on the inner surface of the groove; Coating the copper paste and the composite silver paste in the first protective layer of the groove in an alternating order, and performing a pre-curing treatment after coating the copper paste or the composite silver paste until the copper paste and the composite silver paste fill the groove, and then performing a second curing treatment to obtain a composite core with copper layers and composite silver layers alternately stacked; The composite silver paste is coated on the surface of the composite core away from the substrate, and then the composite core is laminated with the solar cell sheet to be metallized, and then a third curing treatment is performed to form a second protective layer, and the substrate is removed to obtain a composite electrode; The composite silver paste comprises the following components in parts by weight: 60 to 80 parts of silver powder, 0.1 to 5 parts of tin-nickel alloy powder, 10 to 40 parts of organic carrier, and 0.1 to 1 part of antioxidant.

2. The preparation method according to claim 1, characterized in that: The mass ratio of tin to nickel in the tin-nickel alloy powder is 3 / (1-2).

3. The preparation method according to claim 1, characterized in that: The particle size of the tin-nickel alloy powder is 1 to 6 μm.

4. The preparation method according to claim 1, characterized in that: The silver powder is composed of spherical silver powder and flaky silver powder in a mass ratio of (0.5-1.5) / 3.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The organic carrier is selected from at least one of epoxy resin, phenolic resin, ethyl cellulose and acrylic resin; And / or, the antioxidant is selected from at least one of polyvinyl pyrrolidone, 2,6-di-tert-butyl-p-cresol, and ascorbic acid.

6. The preparation method according to any one of claims 1 to 4, characterized in that: The thickness of the first protective layer is 0.5 to 5 μm; And / or, the thickness of the second protective layer is 0.5-5 μm; and / or, the thickness of the composite silver layer in the composite core is 0.5 to 5 μm; And / or, the groove has a width of 10 to 40 μm and a depth of 20 to 60 μm.

7. The preparation method according to claim 1, characterized in that: Before the step of coating the composite silver paste on the groove wall of the groove, the method further includes: performing surface oleophobic treatment on the groove wall of the groove.

8. A composite electrode, characterized in that: The composite electrode is prepared by the preparation method according to any one of claims 1 to 7.

9. A solar cell, characterized in that: The solar cell comprises the composite electrode according to claim 8.