A bimetallic oxide semiconductor gas-sensitive material, preparation method and application thereof
By doping CeO2 and MOx components in metal oxide semiconductor gas-sensitive materials, combined with binders and sol-gel methods, the problems of poor selectivity, low sensitivity and stability of existing materials have been solved, and the detection of ethyl acetate gas has been achieved. The high response value and fast recovery time are suitable for the development of high-precision sensors.
Patent Information
- Application Number
- CN202410488715.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-23
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-04-23
AI Technical Summary
Existing metal oxide semiconductor gas-sensitive materials have poor gas selectivity, low sensitivity, and poor stability, making it difficult to effectively identify and use them for a long time in high-precision and high-sensitivity application scenarios.
Dual metal oxide semiconductor gas-sensitive materials are used, including MOx and CeO2, which are combined by doping or forming a heterojunction. By adding a binder to the precursor, the two components are evenly and tightly combined to enhance sensing. response value, and composite materials were prepared by sol-gel method to improve surface oxygen vacancies and electron transport capabilities.
It achieves super response value and fast recovery time to ethyl acetate gas, improves the accuracy and stability of the sensor, and is suitable for mass production and actual detection.
Smart Images

Figure CN118329980B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of gas sensors, and in particular to a bimetallic oxide semiconductor gas-sensitive material, a preparation method and application thereof in ethyl acetate gas detection. Background Art
[0002] Ethyl acetate (EA) is a common volatile organic compound pollutant, which is widely present in industrial waste gas such as coating, coking, non-ferrous metals, and building materials. Although ethyl acetate is generally considered to be of low toxicity, its harm to the human body should not be underestimated. Long-term exposure to ethyl acetate can cause irritation of the eyes, nose, and throat, and even cause corneal opacity, secondary anemia, and leukocytosis. Secondly, in the medical field, ethyl acetate can be used as a trace biomarker for colorectal cancer and gastric cancer, because ethyl acetate can be detected in the patient's exhaled gas (concentration exceeding 1ppm), so it can be used for non-invasive early screening of such diseases. In addition, ethyl acetate is flammable and explosive, and it will cause an explosion when it exceeds a certain concentration in the atmosphere. China's (GBZ2-2002) "Occupational Exposure Limits for Hazardous Substances in the Workplace" stipulates that the maximum allowable concentration of ethyl acetate vapor in the air is less than 300mg / m3 (76.3ppm). Therefore, selective detection of ethyl acetate at or below the ppm level is of great significance for environmental monitoring, food safety, and disease diagnosis.
[0003] With the improvement of safety and environmental awareness, people have also put forward higher requirements for gas sensors. Traditional large-scale gas chromatography is not only expensive but also not suitable for field scenarios. Lightweight, fast and low-cost sensors have become a new demand. Compared with other gas-sensitive materials, metal oxide semiconductor (MOS) sensors stand out among many gas-sensitive materials for their lightness, easy integration, low cost and simple preparation methods. Commonly used MOS gas-sensitive materials are divided into n-type and p-type materials, including ZnO, SnO2, Fe2O3, MoO3, CeO2, NiO and Cu2O, etc. The wide band gap of these materials gives them a full spectrum of electronic properties (insulation + semiconductor). The performance of MOS is usually greatly affected by the size of the material, especially at the nanoscale. Due to the nano effect, the material will show unique properties. For example, the electrical properties will change significantly, thus forming a good gas-sensitive material, and the nano effect makes them have better stability and fast response under high temperature or harsh environment, which is of great significance in practical work. There are still some problems with the existing MOS-based resistive sensors. Since the response of its resistance change comes from the gain and loss of electrons caused by the redox reaction between the sensing material and the target gas, the response gas is not single. Many gases with similar redox properties and close structures will respond to the same sensing material, making it difficult for the sensing material to distinguish these gases, which causes great trouble in identifying a single gas. This can easily cause misjudgment of the sensor in practical applications. As gas sensing materials are increasingly used in various scenarios, people's performance requirements for the required materials have also increased. Taking ethyl acetate sensors as an example, the detection limits of ethyl acetate sensing materials reported so far are all at the ppm level and the response values are almost all less than 100, which makes ethyl acetate not applicable as a biomarker in the scenario of exhaled breath detection. For this trace detection application scenario, ultra-low detection limits and highly sensitive responses are the key. Secondly, various application scenarios also put forward higher requirements on the short-term repeatability, long-term stability and ability to resist environmental interference of materials.
[0004] Through the above analysis, the problems and defects of the prior art are as follows:
[0005] (1) Metal oxide semiconductor gas-sensitive materials have poor selectivity for gases and usually show a certain response to multiple gases of the same category, making it difficult to distinguish between multiple similar gases.
[0006] (2) Metal oxide semiconductor gas-sensitive materials have low sensitivity and low response values, and are not suitable for certain application scenarios that require high precision and high sensitivity.
[0007] (3) Metal oxide semiconductor gas-sensitive materials usually have poor stability. After multiple tests, it is difficult to restore the material to its original state, resulting in performance degradation.
[0008] Therefore, it is of great significance to further develop gas-sensitive materials with high response, high sensitivity, stability and selectivity. Summary of the invention
[0009] In view of the problems existing in the prior art, the present invention provides a bimetallic oxide semiconductor gas-sensitive material, a preparation method and application thereof in ethyl acetate gas detection.
[0010] The present invention adopts the following technical solution:
[0011] A double metal oxide semiconductor gas-sensitive material comprises two components, MOx and CeO2, wherein M is Fe, Ni, Mn, Co, Ti, Cu or Zn, and the two components are uniformly and tightly combined together by doping or forming a heterojunction, and the molar ratio of MOx to CeO2 is 1:1-10:1.
[0012] Preferably, by adding a binder to the precursor, the two components are evenly and tightly combined together, and the MOx and CeO2 components interact strongly, and the sensing response value is enhanced through electron transfer during the reaction.
[0013] The present invention also provides a method for preparing a bimetallic oxide semiconductor gas-sensitive material, comprising the following steps:
[0014] (1) Preparation of precursor: A certain molar ratio of cerium nitrate hexahydrate, the corresponding nitrate of MOx and citric acid are dissolved in deionized water, and the three solutions are mixed. After being fully stirred, the mixture is evaporated in a water bath at 50-99°C to a gelatinous state. The gelatinous substance is then transferred to an oven, foamed and dried at 60-180°C, collected and ground using an agate mortar to obtain a precursor of the composite material.
[0015] (2) Precursor annealing: The precursor powder is transferred to a muffle furnace, heated at a rate of 6°C / min, and annealed at 250-700°C for 2-12 hours. After annealing, the powder is ground and collected again to obtain a Ce-MO composite gas-sensitive material.
[0016] The single-component materials MOx and CeO2 used for comparison can also be prepared by this method by directly calcining the corresponding nitrates in a muffle furnace.
[0017] Preferably, the molar ratio of the cerium nitrate and the corresponding nitrate of MOx in step (1) is 1:5-10:1; more preferably 1:1-10:1; most preferably 7:1.
[0018] Preferably, the citric acid solution in step (1) is a binder, and the molar ratio of the citric acid solution to the total amount of nitrate is 1:2-3:1, more preferably 1:2-2:1; most preferably 1:1-2:1.
[0019] Preferably, the stirring process in step (1) lasts for more than 2 hours to ensure that the solution is evenly mixed.
[0020] Preferably, the water bath evaporation process in step (1) plays an important role in the formation of the colloid. Preferably, the water bath temperature is 60-90°C and the time is 3-8 hours. More preferably, the hydrothermal temperature is 65-85°C and the time is 4-6 hours, until the sample becomes a viscous gel and then transferred for drying.
[0021] Preferably, in the drying process in step (1), the colloidal substance is transferred to an oven and foamed and dried at 60-180°C. The drying temperature is crucial to the process of colloid foaming. Too low a temperature will lead to incomplete foaming and affect the bonding degree of the two-component oxide. Too high a temperature will cause the sample to burn directly. The drying temperature is further preferably 80-160°C, and most preferably 90-130°C.
[0022] Preferably, the temperature of the oven during the step (1) cannot be lower than the water bath temperature, and is usually 30° C. higher than the water bath temperature, which is the best, to achieve the best foaming and drying effect.
[0023] Preferably, in step (2), the precursor powder is transferred to a muffle furnace, the temperature is increased at 6°C / min, and annealing is performed at 250-700°C for 2-12 hours. More preferably, the temperature is increased at 6°C / min and annealing is performed at 350-600°C for 3-10 hours. Most preferably, the temperature is increased at 6°C / min and annealing is performed at 400-550°C for 4-8 hours.
[0024] Preferably, the products obtained in step (1) and step (2) are ground into fine powder. Grinding the product in step (1) helps the annealing process to be more thorough, and grinding the product in step (2) helps to collect and make the sensor sheet.
[0025] Another object of the present invention is to provide a gas-sensitive material for ethyl acetate gas detection, wherein the material is a bimetallic oxide composite of MOx and cerium oxide (CeO2), and the two components are evenly and tightly combined by adding a binder to the precursor, and two bonding modes of doping and heterojunction are included. Thanks to the in-situ synthesis process of the composite material, the two components have a strong interaction, and in the process of dynamic detection of the target gas, the electron transmission capacity increases exponentially through the redox reaction, which greatly improves the sensing performance.
[0026] The composite gas-sensitive material of the present invention exhibited an ultra-strong response value (Ra / Rg) of up to 300,000 and a recovery time of nearly three seconds in an experiment of dynamically detecting ethyl acetate gas. The response value exceeded that of almost all the chemical resistance gas sensors reported so far, showing broad application prospects in the field of gas sensing.
[0027] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows:
[0028] In order to solve the problem that the response value of traditional sensors is not high and the static gas distribution experiment is difficult to apply to actual scenarios, the present invention prepares the Ce-MO bimetallic oxide gas-sensitive material by the sol-gel method. After the material is composited, its surface has more surface oxygen vacancies, which is more conducive to the formation of surface active oxygen; and CeO2 and MO X The two components are tightly bound and interact significantly with each other. During the reaction process, they can enhance the electron transmission capability, showing super strong response to target gas detection, greatly improving the sensing accuracy of the sensor, laying a good foundation for the development of new metal oxide semiconductors, and providing new possibilities for the development of high-precision integrated sensors.
[0029] As auxiliary evidence of the inventiveness of the claims of the present invention, it is also reflected in the following important aspects:
[0030] (1) The expected benefits after the transformation of the technical solution of the present invention are as follows: Since the sensing material is low-cost, easy to synthesize and inexpensive, it is suitable for mass production and can be used in MEMS technology combined with integrated circuits to form an integrated sensing microsystem, providing a basis and possibility for the development of new portable, fast and compact gas sensing equipment.
[0031] (2) The technical solution of the present invention fills the technical gap in the industry at home and abroad: As of the date of writing of the present invention, there has been no report on a composite metal oxide gas sensing material with super-strong gas sensitive response (200ppm, Ra / Rg≈300000) for detecting ethyl acetate under dynamic gas distribution conditions. The technical solution proposed by the present invention realizes the preparation of super-strong gas sensitive catalysts, and has good stability, which can be used for actual detection.
[0032] (3) The technical solution of the present invention solves a technical problem that people have been eager to solve but have never been able to solve: metal oxide semiconductor gas-sensitive materials have always been limited by problems such as low response value and poor reuse rate. The present invention achieves a gas-sensitive response with an ultra-high response value, greatly improving the accuracy of detection, and has the characteristics of rapid recovery and good stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1This is the XRD diagram of the Fe-Ce-O composite gas-sensitive material synthesized in Example 1 of the present invention (XRD is the abbreviation of X-ray diffraction, i.e. X-ray diffraction), wherein the subscripts of the Fe element and the Ce element represent the molar proportions of different components.
[0034] Figure 2 This is a microscopic morphology image (TEM image, TEM is the abbreviation of Transmission Electron Microscope) of the Fe-Ce-O composite gas-sensitive material synthesized in Example 1 of the present invention.
[0035] Figure 3 This is a microscopic morphology image (SEM image, SEM is the abbreviation of Scanning Electron Microscope) of the Fe-Ce-O composite gas-sensitive material synthesized in Example 1 of the present invention.
[0036] Figure 4 This is a single response curve of the Fe-Ce-O composite gas-sensitive material synthesized in Example 1 of the present invention to detect 200 ppm ethyl acetate gas.
[0037] Figure 5 This is the response diagram of the Fe-Ce-O composite gas-sensitive material synthesized in Example 1 of the present invention when detecting 10ppb-200ppm ethyl acetate gas concentration gradient.
[0038] Figure 6 This is the long-term stability response diagram of the Fe-Ce-O composite gas-sensitive material synthesized in Example 1 of the present invention in detecting 200 ppm ethyl acetate gas (tested every two days for 16 days). DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0040] In order to enable those skilled in the art to fully understand how to implement the present invention in detail, this section is an explanatory embodiment that expands and describes the technical solution of the claims.
[0041] Example 1.
[0042] Preparation of Fe-Ce-O precursor: The molar ratio of the raw materials is ferric nitrate: cerium nitrate: citric acid = 7:1:12, totaling 10 g. After mixing, dissolve in 30 ml of deionized water and stir for 2.5 hours to make it fully and evenly mixed. Put the beaker containing the mixed solution into a water bath and evaporate at 80°C for 5 hours to remove a large amount of water, so that the solution in the beaker becomes viscous and colloid. Then transfer the beaker to a 110°C oven for foaming and drying for 12 hours. Collect the obtained product and grind it into fine powder with an agate mortar.
[0043] Preparation of Fe-Ce-O: The precursor product was transferred to a muffle furnace, and the temperature was continuously raised to 500°C at 6°C / min for annealing for 5 hours. After natural cooling, the product was collected and ground with agate to obtain a Fe-Ce-O composite gas-sensitive material. The prepared material was simply characterized, such as Figure 1 , Figure 2 , Figure 3 Shown are XRD, SEM and TEM images respectively.
[0044] Performance test of gas-sensitive materials: Take 0.015g of the above-synthesized composite gas-sensitive material and dissolve it in 400uL of deionized water. Place the sample in an ultrasonic machine and sonicate for 5 minutes to disperse it evenly in the water. Use a pipette to take 5ul of the dispersed sample solution and evenly coat it on the resistive sensor sheet (4mm×8mm). The sensor sheet consists of two interdigitated gold (Au) electrodes on the surface of the silicon dioxide (SiO2) substrate. The interdigitated area is the coating area of the sensing material. After the sensor sheet is naturally dried, a layer of composite gas-sensitive material is coated on the surface of the sensor sheet. Place the sensor sheet on a program-controlled temperature heating table, heat it to 350°C, connect it to a resistance testing machine, and introduce air, 200ppm ethyl acetate gas and air in turn at a rate of 3L / min to obtain a response value change curve. The gas-sensitive performance is as follows. Figure 4 , Figure 5 , Figure 6 As shown in Figure 2, the material exhibits good sensing performance for ethyl acetate gas. Figure 4 It can be seen that the response value for 200ppm ethyl acetate reaches more than 300000, and has a response time of 63S and an ultra-fast recovery time of less than 5S; Figure 5 It can be found that the minimum detection limit can reach 10ppb, and even at the minimum detection limit, a response value of 4.8 can still be achieved, and the response value in the concentration range of 10ppb-200ppm has a good linear gradient; Figure 6 The long-term stability also shows that the material has good stability, providing a basis for practical applications.
[0045] Example 2.
[0046] Preparation of Ni-Ce-O precursor: The molar ratio of the raw materials is nickel nitrate: cerium nitrate: citric acid = 7:1:12, totaling 10 g. After mixing, dissolve in 30 ml of deionized water and stir for 2.5 hours to make it fully and evenly mixed. Put the beaker containing the mixed solution into a water bath and evaporate at 80°C for 5 hours to remove a large amount of water, so that the solution in the beaker becomes viscous and colloid. Then transfer the beaker to a 110°C oven for foaming and drying for 12 hours. Collect the obtained product and grind it into fine powder with an agate mortar.
[0047] Preparation of Ni-Ce-O: The precursor product was transferred to a muffle furnace, and the temperature was continuously raised to 500 °C at 6 °C / min for annealing for 5 hours. After natural cooling, the product was collected and ground with agate to obtain a Ni-Ce-O composite gas-sensitive material.
[0048] Performance test of gas-sensitive materials: Take 0.015g of the above-synthesized composite gas-sensitive material and dissolve it in 400ul of deionized water. Place the sample in an ultrasonic machine for 5min to make it dispersed evenly in the deionized water. Then use a pipette to take 5ul of the dispersed sample solution and evenly coat it on the resistive sensor sheet. The (4mm×8mm) sensor sheet consists of two interdigitated gold (Au) electrodes on the surface of the silicon dioxide (SiO2) substrate. The interdigitated area is the coating area of the sensing material. After the sensor sheet is naturally dried, a layer of composite gas-sensitive material is coated on the surface of the sensor sheet. Place the sensor sheet on a program-controlled temperature heating table, heat it to 350℃, connect it to the resistance testing machine, and introduce air, 200ppm ethyl acetate gas and air in turn at a rate of 3L / min to obtain the response value change curve. The results show that the response value of the material to 200ppm ethyl acetate is 6550, the response time is 139s, and the recovery time is 87s. The sensing performance is slightly lower than that of the Fe-Ce-O material in Example 1.
[0049] Example 3.
[0050] Preparation of Mn-Ce-O precursor: The molar ratio of the raw materials is manganese nitrate: cerium nitrate: citric acid = 7:1:12, totaling 10 g. After mixing, dissolve in 30 ml of deionized water and stir for 2.5 hours to make it fully and evenly mixed. Put the beaker containing the mixed solution into a water bath and evaporate at 80°C for 5 hours to remove a large amount of water, so that the solution in the beaker becomes viscous and colloid. Then transfer the beaker to a 110°C oven for foaming and drying for 12 hours. Collect the obtained product and grind it into fine powder with an agate mortar.
[0051] Preparation of Mn-Ce-O: The precursor product was transferred to a muffle furnace, and the temperature was continuously raised to 500 °C at 6 °C / min for annealing for 5 hours. After natural cooling, the product was collected and ground with agate to obtain a Mn-Ce-O composite gas-sensitive material.
[0052] Performance test of gas-sensitive materials: Take 0.015g of the above-synthesized composite gas-sensitive material and dissolve it in 400ul of deionized water. Place the sample in an ultrasonic machine for 5min to make it dispersed evenly in water. Then use a pipette to take 5ul of the dispersed sample solution and evenly coat it on the resistive sensor sheet. The (4mm×8mm) sensor sheet consists of two interdigitated gold (Au) electrodes on the surface of the silicon dioxide (SiO2) substrate. The interdigitated area is the coating area of the sensing material. After the sensor sheet is naturally dried, a layer of composite gas-sensitive material is coated on the surface of the sensor sheet. Place the sensor sheet on a program-controlled temperature heating table, heat it to 350℃, connect it to the resistance testing machine, and introduce air, 200ppm ethyl acetate gas and air in turn at a rate of 3L / min to obtain the response value change curve. The results show that the response value of the material to 200ppm ethyl acetate is 1870, the response time is 215s, and the recovery time is 110s. The sensing performance is slightly lower than that of the Fe-Ce-O material in Example 1.
[0053] Example 4.
[0054] Preparation of Co-Ce-O precursor: The molar ratio of the raw materials is cobalt nitrate: cerium nitrate: citric acid = 7:1:12, totaling 10 g. After mixing, dissolve in 30 ml of deionized water and stir for 2.5 hours to make it fully and evenly mixed. Put the beaker containing the mixed solution into a water bath and evaporate at 80°C for 5 hours to remove a large amount of water, so that the solution in the beaker becomes viscous and colloid. Then transfer the beaker to a 110°C oven for foaming and drying for 12 hours. Collect the obtained product and grind it into fine powder with an agate mortar.
[0055] Preparation of Co-Ce-O: The precursor product was transferred to a muffle furnace, and the temperature was continuously raised to 500 °C at 6 °C / min for annealing for 5 h. After natural cooling, the product was collected and ground with agate to obtain a Co-Ce-O composite gas-sensitive material.
[0056] Performance test of gas-sensitive materials: Take 0.015g of the above-synthesized composite gas-sensitive material and dissolve it in 400ul of deionized water. Place the sample in an ultrasonic machine for 5min to make it dispersed evenly in water. Then use a pipette to take 5ul of the dispersed sample solution and evenly coat it on the resistive sensor sheet. The (4mm×8mm) sensor sheet consists of two interdigitated gold (Au) electrodes on the surface of the silicon dioxide (SiO2) substrate. The interdigitated area is the coating area of the sensing material. After the sensor sheet is naturally dried, a layer of composite gas-sensitive material is coated on the surface of the sensor sheet. Place the sensor sheet on a program-controlled temperature heating table, heat it to 350℃, connect it to the resistance testing machine, and introduce air, 200ppm ethyl acetate gas and air in turn at a rate of 3L / min to obtain the response value change curve. The results show that the response value of the material to 200ppm ethyl acetate is 3340, the response time is 177s, and the recovery time is 81s. The sensing performance is slightly lower than that of the Fe-Ce-O material in Example 1.
[0057] Example 5.
[0058] Preparation of Ti-Ce-O precursor: The molar ratio of the raw materials is titanium nitrate: cerium nitrate: citric acid = 7:1:12, totaling 10 g. After mixing, dissolve in 30 ml of deionized water and stir for 2.5 hours to make it fully and evenly mixed. Put the beaker containing the mixed solution into a water bath and evaporate at 80°C for 5 hours to remove a large amount of water, so that the solution in the beaker becomes viscous and colloid. Then transfer the beaker to a 110°C oven for foaming and drying for 12 hours. Collect the obtained product and grind it into fine powder with an agate mortar.
[0059] Preparation of Ti-Ce-O: The precursor product was transferred to a muffle furnace, and the temperature was continuously raised to 500 °C at 6 °C / min for annealing for 5 hours. After natural cooling, the product was collected and ground with agate to obtain a Ti-Ce-O composite gas-sensitive material.
[0060] Performance test of gas-sensitive materials: Take 0.015g of the above-synthesized composite gas-sensitive material and dissolve it in 400ul of deionized water. Place the sample in an ultrasonic machine for 5min to make it dispersed evenly in water. Then use a pipette to take 5ul of the dispersed sample solution and evenly coat it on the resistive sensor sheet. The (4mm×8mm) sensor sheet consists of two interdigitated gold (Au) electrodes on the surface of the silicon dioxide (SiO2) substrate. The interdigitated area is the coating area of the sensing material. After the sensor sheet is naturally dried, a layer of composite gas-sensitive material is coated on the surface of the sensor sheet. Place the sensor sheet on a program-controlled temperature heating table, heat it to 350℃, connect it to the resistance testing machine, and introduce air, 200ppm ethyl acetate gas and air in turn at a rate of 3L / min to obtain the response value change curve. The results show that the response value of the material to 200ppm ethyl acetate is 3730, the response time is 149, and the recovery time is 96s. The sensing performance is slightly lower than that of the Fe-Ce-O material in Example 1.
[0061] Example 6.
[0062] Preparation of Cu-Ce-O precursor: The molar ratio of the raw materials is copper nitrate: cerium nitrate: citric acid = 7:1:12, totaling 10 g. After mixing, dissolve in 30 ml of deionized water and stir for 2.5 hours to make it fully and evenly mixed. Put the beaker containing the mixed solution into a water bath and evaporate at 80°C for 5 hours to remove a large amount of water, so that the solution in the beaker becomes viscous and colloid. Then transfer the beaker to a 110°C oven for foaming and drying for 12 hours. Collect the obtained product and grind it into fine powder with an agate mortar.
[0063] Preparation of Cu-Ce-O: The precursor product was transferred to a muffle furnace, and the temperature was continuously raised to 500 °C at 6 °C / min for annealing for 5 hours. After natural cooling, the product was collected and ground with agate to obtain a Cu-Ce-O composite gas-sensitive material.
[0064] Performance test of gas-sensitive materials: Take 0.015g of the above-synthesized composite gas-sensitive material and dissolve it in 400ul of deionized water. Place the sample in an ultrasonic machine for 5min to make it dispersed evenly in water. Then use a pipette to take 5ul of the dispersed sample solution and evenly coat it on the resistive sensor sheet. The (4mm×8mm) sensor sheet consists of two interdigitated gold (Au) electrodes on the surface of the silicon dioxide (SiO2) substrate. The interdigitated area is the coating area of the sensing material. After the sensor sheet is naturally dried, a layer of composite gas-sensitive material is coated on the surface of the sensor sheet. Place the sensor sheet on a program-controlled temperature heating table, heat it to 350℃, connect it to the resistance testing machine, and introduce air, 200ppm ethyl acetate gas and air in turn at a rate of 3L / min to obtain the response value change curve. The results show that the response value of the material to 200ppm ethyl acetate is 12540, the response time is 99s, and the recovery time is about 36s. The sensing performance is slightly lower than that of the Fe-Ce-O material in Example 1.
[0065] Example 7.
[0066] Preparation of Zn-Ce-O precursor: The molar ratio of the raw materials is zinc nitrate: cerium nitrate: citric acid = 7:1:12, totaling 10 g. After mixing, dissolve in 30 ml of deionized water and stir for 2.5 hours to make it fully and evenly mixed. Put the beaker containing the mixed solution into a water bath and evaporate at 80°C for 5 hours to remove a large amount of water, so that the solution in the beaker becomes viscous and colloid. Then transfer the beaker to a 110°C oven for foaming and drying for 12 hours. Collect the obtained product and grind it into fine powder with an agate mortar.
[0067] Preparation of Zn-Ce-O: The precursor product was transferred to a muffle furnace, and the temperature was continuously raised to 500 °C at 6 °C / min for annealing for 5 hours. After natural cooling, the product was collected and ground with agate to obtain a Zn-Ce-O composite gas-sensitive material.
[0068] Performance test of gas-sensitive materials: Take 0.015g of the above-synthesized composite gas-sensitive material and dissolve it in 400ul of deionized water. Place the sample in an ultrasonic machine for 5min to make it dispersed evenly in water. Then use a pipette to take 5ul of the dispersed sample solution and evenly coat it on the resistive sensor sheet. The (4mm×8mm) sensor sheet consists of two interdigitated gold (Au) electrodes on the surface of the silicon dioxide (SiO2) substrate. The interdigitated area is the coating area of the sensing material. After the sensor sheet is naturally dried, a layer of composite gas-sensitive material is coated on the surface of the sensor sheet. Place the sensor sheet on a program-controlled temperature heating table, heat it to 350℃, connect it to the resistance testing machine, and introduce air, 200ppm ethyl acetate gas and air in turn at a rate of 3L / min to obtain the response value change curve. The results show that the response value of the material to 200ppm ethyl acetate is 8120, the response time is 112s, and the recovery time is 73s. The sensing performance is slightly lower than that of the Fe-Ce-O material in Example 1.
Claims
1. An application of a bimetallic oxide semiconductor gas-sensitive material, characterized in that: Applied to the detection of ethyl acetate gas, the bimetallic oxide semiconductor gas-sensitive material comprises two components, MOx and CeO2, where M is Fe, Ni, Mn, Co, Ti or Zn, and the two components are uniformly and closely combined together by doping or forming a heterojunction, and the molar ratio of MOx to CeO2 is 1:1-10:1; The method for preparing the bimetallic oxide semiconductor gas-sensitive material comprises the following steps: (1) Preparation of precursor: a certain molar ratio of cerium nitrate hexahydrate, the corresponding nitrate of MOx and citric acid are dissolved in deionized water, stirred and mixed thoroughly, and then evaporated to a colloid in a water bath at 50-100°C. The colloid is then transferred to an oven, foamed and dried at 60-180°C to obtain a precursor of the composite material. (2) Annealing: Transfer the precursor powder to a muffle furnace and anneal it at 250-700°C for 2-12 hours to obtain a bimetallic oxide semiconductor gas-sensitive material.
2. The use of the bimetallic oxide semiconductor gas-sensitive material according to claim 1, characterized in that: By adding a binder to the precursor, the two components are evenly and tightly combined together, and the MOx and CeO2 components interact strongly, enhancing the sensing response value through electron transfer during the reaction.
3. The use of the bimetallic oxide semiconductor gas-sensitive material according to claim 1, characterized in that: The amount of citric acid used in step (1) is 1-2 times the total amount of nitrate.
4. The use of the bimetallic oxide semiconductor gas-sensitive material according to claim 1, characterized in that: The stirring and mixing process in step (1) is continued for more than 2 hours to ensure that the two components are fully and evenly mixed.
5. The use of the bimetallic oxide semiconductor gas-sensitive material according to claim 1, characterized in that: In step (1), the water bath temperature must be maintained above 60°C.
6. The use of the bimetallic oxide semiconductor gas-sensitive material according to claim 1, characterized in that: The temperature of the oven during the step (1) is not lower than the water bath temperature.
7. The use of the bimetallic oxide semiconductor gas-sensitive material according to claim 1, characterized in that: In step (2), the precursor powder is transferred to a muffle furnace, the temperature is raised at a rate of 6°C / min, and annealed at 250-700°C for 2-12 hours.