A bimetallic solid-liquid composite casting molding device and method

By applying an electric field to the bimetal interface during the lost foam casting process to control the formation and distribution of intermetallic compounds, the problem of excessive brittle intermetallic compounds at the interface and uneven solidification structure in bimetal castings is solved, and the bonding strength and mechanics are improved. performance, simplifying the process and reducing costs.

CN118455492BActive Publication Date: 2024-10-22HUAZHONG UNIV OF SCI & TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410563423.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-08
Publication Date
2024-10-22
Estimated Expiration
2044-05-08

AI Technical Summary

Technical Problem

In the process of preparing bimetal castings, lost foam casting technology has problems such as excessive brittle intermetallic compounds at the interface, uneven solidification structure and oxidation inclusions, resulting in low bonding strength and limiting the development and application of bimetallic materials.

Method used

A bimetallic solid-liquid composite casting molding device and method is used to apply a DC or pulsed electric field to the bimetal interface by using an electric field generating device during the lost foam casting process to control the formation and distribution of intermetallic compounds, optimize the interface structure, and reduce oxidation membrane influence.

Benefits of technology

It can effectively reduce the generation of hard and brittle compounds, enhance the bonding strength of the interface, simplify the process, reduce costs, and improve the structural integrity and mechanical properties of bimetal castings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118455492B_ABST
    Figure CN118455492B_ABST
Patent Text Reader

Abstract

The present invention proposes a bimetallic solid-liquid composite casting molding device and method, the molding device includes a sand box component, a composite model component and an electric field generating device, the sand box component includes a sand box, dry sand and a film; the composite model component includes a pouring cup, a runner foam model, a casting foam model and a solid insert, the runner foam model is connected to the casting foam model and is arranged in the dry sand, the pouring cup is connected to the runner foam model, and the solid insert is embedded in the casting foam model; the electric field generating device includes a first electrode, a second electrode and a power supply device, the first electrode is connected to the solid insert, the second electrode is embedded in the casting foam model, and the two electrodes are respectively connected to the power supply device through a cable. The entire device has a simple structure, and only needs to add an electrification process in the lost foam casting process. The process is simple and easy to implement. The use of electric field to control interface bonding can effectively control the formation of intermetallic compounds at the interface and enhance the bonding strength of the interface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of casting, and in particular to a bimetallic solid-liquid composite casting molding device and method. Background Art

[0002] With the continuous development of modern industry, the comprehensive performance requirements for parts are getting higher and higher. The use of a single material can no longer meet the requirements. Therefore, new materials need to be developed to meet the needs of practical engineering applications. Bimetallic materials are a new type of composite material prepared by metallurgically bonding two different metal materials at the interface through a composite molding method. The advantage of bimetallic materials is that they can maintain the independence of the properties of the two alloys and achieve the complementary advantages of the two alloys as a whole. Compared with single material alloys, they have better comprehensive performance and have broad application prospects in the fields of automobiles, weapons and equipment, and aviation.

[0003] There are many preparation processes and methods for bimetallic materials, such as welding, plastic forming and casting. Lost foam casting has unique advantages in the preparation of bimetallic materials. It is a near-net forming process with large structural design freedom, high dimensional accuracy and high material utilization. The mold of lost foam casting is loose sand without binder, and the cooling speed of the casting is slow, which is conducive to metallurgical bonding. Solid-liquid composite lost foam casting can fix the prefabricated solid metal parts as inlays in the foam mold. The operation is simple and the interface formation is relatively easy to control. Lost foam casting has broad development prospects and application potential in the preparation of bimetallic materials.

[0004] However, there are still some problems in the process of preparing bimetallic castings using the lost foam casting technology.

[0005] During the lost foam casting process, the heat input is large, and there is more melting on the surface of the solid inlay. The two metals can be infinitely miscible in the liquid state, resulting in the generation of a large number of continuous hard and brittle intermetallic compounds at the interface, which is very easy to form cracks during the deformation process and reduce the bonding strength. At the same time, due to the large temperature difference between the inlay and the molten metal, a temperature gradient perpendicular to the surface of the solid inlay will be formed in the interface area during the solidification process, and the formed intermetallic compound structure is coarse and uneven. In addition, the dense oxide film on the surface of the solid inlay will not only hinder the metallurgical bonding reaction of the interface, but also be difficult to remove, and will form inclusion defects in the interface. The above problems will reduce the interfacial bonding of bimetallic materials, have an extremely adverse effect on the mechanical properties of the interfacial bonding, and greatly limit the development and application of bimetallic materials in lost foam casting.

[0006] In order to solve the problems of more brittle intermetallic compounds in the interface area, coarse and uneven solidification structure, and easy generation of oxide inclusions in the lost foam casting process, the current solutions mainly include adding an intermediate layer and ultrasonic vibration. Adding an intermediate layer can effectively prevent direct contact between the two metals and greatly reduce the generation of hard and brittle intermetallic compounds, but the introduction of the metal interlayer may produce more types of compounds, and the process is complex and difficult to control; ultrasonic vibration can directly act on the interface of the two metals and has a better effect on the regulation of the interface, but the ultrasonic equipment needs to be matched with the solid inlay, and the equipment cost is relatively high. Summary of the invention

[0007] In view of this, the present invention proposes a bimetallic solid-liquid composite casting forming device and method, which can simply, effectively and low-costly control the interface bonding performance of the bimetallic solid-liquid composite casting when forming bimetallic castings.

[0008] The technical solution of the present invention is achieved as follows:

[0009] In a first aspect, the present invention provides a bimetallic solid-liquid composite casting molding device, the molding device comprising a sand box assembly, a composite model assembly and an electric field generating device;

[0010] The sand box assembly includes a sand box, dry sand and a film, wherein the dry sand is filled in the sand box, and the sand box can be vacuumed to allow the film to be tightly attached to the top surface of the sand box;

[0011] The composite model assembly includes a pouring cup, a runner foam model, a casting foam model and a solid insert, the runner foam model is connected to the casting foam model, and both are arranged in dry sand, the pouring cup is arranged on the top surface of the sand box and connected to the runner foam model, and the solid insert is embedded in the casting foam model;

[0012] The electric field generating device includes a first electrode, a second electrode, a cable and a power supply device. The first electrode is connected to one end of the solid insert, and the second electrode is embedded in the casting foam model or the runner foam model. The first electrode and the second electrode are respectively connected to the power supply device through cables.

[0013] On the basis of the above technical solution, preferably, the solid insert is an aluminum metal insert or a magnesium metal insert, and the length of the solid insert extending out of the casting foam model portion is 10 mm to 30 mm.

[0014] Further, preferably, the first electrode and the second electrode are both high temperature resistant graphite electrodes, the first electrode is connected to the upper end of the fixed insert extending out of the casting foam model, and the first electrode is connected to the positive pole of the power supply equipment through a cable, and the second electrode is embedded in the lower end of the casting foam model or the lower end of the runner foam model, and the second electrode is connected to the negative pole of the power supply equipment through a cable.

[0015] Furthermore, preferably, the runner foam model is connected to the lower end of the casting foam model, and the second electrode is embedded in the connection between the runner foam model and the casting foam model.

[0016] On the basis of the above technical solution, preferably, a suction pipe connected to an external negative pressure suction device is provided on the bottom surface of the sand box.

[0017] On the basis of the above technical solution, preferably, the device further comprises a vibration table, and the sand box is fixedly arranged on the vibration table.

[0018] In a second aspect, the present invention discloses a bimetallic solid-liquid composite casting method, which utilizes the bimetallic solid-liquid composite casting device described in the first aspect, and comprises the following steps:

[0019] S1, placing the casting foam model and the runner foam model connected as one in a sand box, embedding a solid insert in the casting foam model, installing a first electrode at one end of the solid insert, inserting a second electrode into the casting foam model or the runner foam model, and connecting the first electrode and the second electrode to a power supply device through a cable respectively;

[0020] S2, fill the sand box with dry sand and vibrate it. When the sand box is filled, cover the top surface of the sand box with a film and evacuate the sand box to compact the dry sand in the sand box;

[0021] S3, install a pouring cup on the top of the sand box, so that the pouring cup is connected to the top of the runner foam model;

[0022] S4, pouring molten metal through the pouring cup, the molten metal sequentially melts the runner foam model and the casting foam model, and combines with the solid insert in the cavity formed by the casting foam model and the dry sand;

[0023] S5. After the pouring is completed, when the bimetallic interface reaches 500°C, start the power supply equipment to apply a DC electric field to the solid insert and the metal melt for a certain period of time until the bimetallic interface temperature is lower than 400°C and then turn off the electric field;

[0024] S6. After the molten metal in the sand box solidifies, the sand box vacuum is released, the first electrode and the second electrode are removed, and the runner formed by the runner foam model is removed to obtain a bimetallic casting.

[0025] On the basis of the above technical solution, preferably, the current density applied by the power supply device to the solid insert and the metal melt is 300-500A / cm 2 .

[0026] On the basis of the above technical solution, preferably, the vacuum degree in the sand box is 0.01MPa to 0.07MPa.

[0027] On the basis of the above technical solution, preferably, the power supply device is a DC regulated current and voltage power supply or an electric pulse generator.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) The present invention can effectively control the formation of intermetallic compounds at the interface and optimize their distribution through the action of electric field, thereby reducing the generation of hard and brittle compounds and enhancing the bonding strength of the interface. The entire equipment has a simple structure and only requires an additional power-on process during the lost foam casting process. The process is simple and easy to implement. The use of electric field to control interface bonding is lower in cost and easier to operate than the traditional method of adding an intermediate layer or using ultrasonic vibration.

[0030] (2) By extending the solid insert outside the casting foam model, on the one hand, it can prevent the flow of molten metal from directly impacting the end of the solid insert, causing the solid insert to shift, and on the other hand, it is also convenient to install the electrode.

[0031] (3) The second electrode is embedded at the connection between the pouring foam model and the casting foam model, which can optimize the metal flow characteristics in this area. The electric field will affect the flow state and speed of the molten metal, thereby helping the molten metal to transfer more smoothly from the pouring to the casting foam model and reduce local overheating caused by the impact of the liquid metal. By setting an electric field at the starting point of the molten metal entering the casting foam model, the reaction of the metal interface can be controlled at the initial stage, which helps to form a more uniform and dense intermetallic compound layer on the bonding surface of the bimetallic casting, thereby improving the structural integrity and strength of the overall casting.

[0032] (4) The DC electric field or pulse electric field applied by the present invention will generate Joule heat at the bimetallic interface due to the Peltier effect, reduce the influence of the vertical interface temperature gradient caused by the temperature difference on the solidification structure, prevent the formation of coarse dendrites perpendicular to the interface, and refine the structure. The DC electric field can effectively reduce the dendrite spacing of dendrites growing vertically to the interface, promote the transformation of coarse dendrites to fine equiaxed crystals, and in addition, the DC electric field will reduce the supercooling of the solidification process of the intermetallic compound, increase the nucleation rate, and have the effect of refining the structure. In addition, since electrons will collide with metal atoms under the action of high current density, the DC electric field realizes the disturbance of the metal liquid through the momentum exchange between metal atoms and electrons, produces an undulating effect on the solidification structure, reduces the supercooling of the solidification process of the intermetallic compound, increases the nucleation rate, and realizes the refinement of the interface structure, thereby improving the mechanical properties after the bimetallic interface is combined. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 It is a schematic diagram of the planar structure of the bimetallic solid-liquid composite casting molding device disclosed in the present invention;

[0035] Figure 2 It is a principle diagram of the interface formation of the aluminum / magnesium bimetallic solid-liquid composite casting disclosed in the present invention;

[0036] Reference numerals:

[0037] 1. Sand box assembly; 2. Composite model assembly; 3. Electric field generating device; 11. Sand box; 12. Dry sand; 13. Film; 21. Pouring cup; 22. Runner foam model; 23. Casting foam model; 24. Solid insert; 31. First electrode; 32. Second electrode; 33. Cable; 34. Power supply equipment; 111. Suction tube; 4. Vibrating table. DETAILED DESCRIPTION

[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] like Figure 1 As shown, the present invention discloses a bimetallic solid-liquid composite casting molding device, comprising a sand box component 1, a composite model component 2 and an electric field generating device 3.

[0040] The sand box assembly 1 includes a sand box 11, dry sand 12 and a film 13. The sand box 11 is used as a container for the entire casting device. Its function is to contain the dry sand 12 and the composite model assembly 2 to form a space suitable for casting. The dry sand 12 is filled in the sand box 11 as a supporting material for the model to ensure that the model maintains its shape and stability during the casting process. In the case of vacuum, the film 13 fits tightly to the top surface of the sand box 11 to enhance the structural compactness inside the sand box 11 and reduce the deformation and sand loss of the casting during the molding process.

[0041] The composite model assembly 2 includes a pouring cup 21 , a runner foam model 22 , a casting foam model 23 and a solid insert 24 .

[0042] Among them, the pouring cup 21 is located on the top surface of the sand box 11, and is the entrance for the molten metal to enter the model. Through its connection with the runner foam model 22, the molten metal is smoothly guided. The upper end of the runner foam model 22 is connected to the pouring cup 21, and the lower end is connected to the casting foam model 23, which plays the role of distributing the molten metal to various parts of the casting model. The casting foam model 23 is used to determine the shape and size of the final casting, and the solid insert 24 is embedded in it to form a metallurgical bond between the metals. The solid insert 24 is pre-placed in the casting foam model 23 as a part of the casting, and is a key part of the bimetallic solid-liquid composite casting.

[0043] The electric field generating device 3 includes a first electrode 31, a second electrode 32, a cable 33 and a power supply device 34. The first electrode 31 is connected to one end of the solid insert 24, and the second electrode 32 is embedded in the casting foam model 23 or the runner foam model 22. The first electrode 31 and the second electrode 32 are respectively connected to the power supply device 34 through the cable 33. The power supply device 34 can apply a certain DC electric field to the solid insert 24 and the metal melt, and the application of the electric field can improve the bimetallic interface bonding performance.

[0044] Through the action of the electric field, the formation of intermetallic compounds at the interface can be effectively controlled and their distribution can be optimized, thereby reducing the generation of hard and brittle compounds and enhancing the bonding strength of the interface. The entire equipment has a simple structure and only requires an additional power-on process during the lost foam casting process. The process is simple and easy to implement. Using electric fields to control interface bonding is lower in cost and easier to operate than traditional methods of adding an intermediate layer or using ultrasonic vibration.

[0045] The bimetallic solid-liquid composite casting molding device disclosed in this embodiment can mold many types of bimetallic castings, such as aluminum / magnesium bimetallic castings, aluminum / copper bimetallic castings, aluminum / iron bimetallic castings, aluminum / steel bimetallic castings, etc., and has a wide range of applications.

[0046] This embodiment takes aluminum / magnesium bimetallic castings as an example. When the solid insert 24 is made of aluminum metal, the poured magnesium metal liquid makes the magnesium metal melt wrap the aluminum metal insert; when the solid insert 24 is made of magnesium metal, the poured aluminum metal liquid makes the aluminum metal melt wrap the magnesium metal insert. As a result, in the manufacturing process of bimetallic castings, the most suitable material can be selected according to the use environment and performance requirements of the final product. For example, aluminum metal can be selected as the solid insert 24 in applications that require higher strength and lightness, and magnesium metal can be selected as the solid insert 24 in applications that require better electromagnetic shielding capabilities.

[0047] In this embodiment, the length of the solid insert 24 extending out of the casting foam model 23 is 10 mm to 30 mm. This configuration helps to maintain the stability of the position of the solid insert 24 after the molten metal is injected into the cavity formed by the casting foam model 23 and the dry sand 12.

[0048] Specifically, if the two ends of the insert are flush with the casting foam model 23, the flow of molten metal will directly impact the end of the solid insert 24, causing the solid insert 24 to shift, thereby causing the bimetallic casting to fail to meet the design requirements after molding. At the same time, it can also avoid the diffusion of the sand mold due to the impact of the end of the solid insert 24 on the dry sand 12 during the movement of the solid insert 24.

[0049] Secondly, the extended portion of the solid insert 24 also facilitates the installation and stable connection of the electrode. If the end of the insert is flush with the model, the electrode connection may not be strong enough, which will affect the effective transmission of the electric field and the electrical stability of the overall casting process.

[0050] In some preferred embodiments, in order to protect the sand core from being broken or deformed during the pouring process, it is necessary to brush high-temperature resistant paint on the foam model. In order to prevent the paint from flowing into between the solid insert 24 and the foam model, the solid insert 24 needs to be extended out of the model, and the gaps where the solid insert 24 contacts the upper and lower surfaces of the model need to be filled with foam particles.

[0051] In some implementation modes, the upper end extends 2-4 cm to facilitate the installation of graphite electrodes, and the lower end extends 0-0.5 cm.

[0052] As some preferred embodiments, the first electrode 31 and the second electrode 32 are both high-temperature resistant graphite electrodes. Since graphite has excellent electrical conductivity and extremely high high-temperature resistance, during the high-temperature casting process, the graphite electrode can maintain structural stability and is not easily corroded or melted, thereby ensuring stable application of the electric field.

[0053] The first electrode 31 is connected to the upper end of the solid insert 24 extending out of the casting foam model 23, and the first electrode 31 is connected to the positive electrode of the power supply device 34 through the cable 33. The second electrode 32 is embedded in the lower end of the casting foam model 23 or the lower end of the runner foam model 22, and the second electrode 32 is connected to the negative electrode of the power supply device 34 through the cable 33. With the above structure, the current passes through the solid insert 24 and the liquid metal to form an electric field passing through the entire casting foam model 23, which promotes the optimization of the metal interface within the entire casting range.

[0054] In addition, the second electrode 32 is positioned so that the electric field can evenly cover the entire casting area, which helps to ensure uniformity and consistency of the microstructure inside the entire casting. The uniform electric field can optimize the distribution of intermetallic compounds, reduce stress concentration caused by compound aggregation, reduce the risk of crack formation, and significantly improve the interface bonding quality and overall performance of the bimetallic casting.

[0055] In this embodiment, the runner foam model 22 is connected to the lower end of the casting foam model 23. Specifically, the upper end of the runner foam model 22 is poured with molten metal by the pouring cup 21. The molten metal instantly vaporizes after passing through the runner foam model 22, and then is guided to the casting foam model 23 along the channel between the model and the dry sand 12. After the molten metal fills the space formed by the casting foam model 23 and the dry sand 12, it is wrapped and combined with the solid insert 24. In some preferred embodiments, the runner foam model 22 and the casting foam model 23 are integrally formed.

[0056] The second electrode 32 is embedded at the connection between the pouring foam model 22 and the casting foam model 23, which can optimize the metal flow characteristics in this area. The electric field will affect the flow state and speed of the molten metal, thereby helping the molten metal to transfer more smoothly from the pouring to the casting foam model 23, reducing local overheating caused by the impact of the molten metal. By setting an electric field at the starting point of the molten metal entering the casting foam model 23, the reaction of the metal interface can be controlled at the initial stage, which helps to form a more uniform and dense intermetallic compound layer on the bonding surface of the bimetallic casting, thereby improving the structural integrity and strength of the overall casting.

[0057] In addition, the second electrode 32 is embedded in the connection between the runner foam model 22 and the casting foam model 23, which can avoid the second electrode 32 being directly embedded in the casting foam model 23. After the casting is formed and the electrode is removed, electrode gaps will remain on the surface of the casting, making the casting incomplete.

[0058] Preferably, a suction pipe 111 connected to an external negative pressure suction device is provided on the bottom surface of the sand box 11. According to this arrangement, when the composite model component 2 is installed in the sand box 11 and the electric field generating device 3 is connected, the sand box 11 is filled with vibrated dry sand 12, a film 13 is affixed, and negative pressure suction is used to evacuate the dry sand 12 in the sand box 11, so that the dry sand 12 tightly wraps the composite model component 2.

[0059] As some preferred embodiments, the molding device further includes a vibration table 4, and the sand box 11 is fixedly arranged on the vibration table 4. The dry sand 12 in the sand box 11 can be vibrated and compacted by the vibration table 4. In some embodiments, before the composite model component 2 is placed in the sand box 11, a certain amount of dry sand 12 can be filled in the sand box 11, and then the composite model component 2 is placed on the dry sand 12, and then the dry sand 12 is filled, so that the filling and compaction of the dry sand 12 can be completed quickly. At the same time, filling a certain amount of dry sand 12 first can support the composite model component 2, which is convenient for positioning the composite model component 2 in the sand box 11.

[0060] The present invention also discloses a bimetallic solid-liquid composite casting method, which comprises the following steps:

[0061] S1. Place the casting foam model 23 and the runner foam model 22 connected as one in a sand box 11, embed a solid insert 24 in the casting foam model 23, install a first electrode 31 at one end of the solid insert 24, insert a second electrode 32 into the casting foam model 23 or the runner foam model 22, and the first electrode 31 and the second electrode 32 are respectively connected to a power supply device 34 through a cable 33.

[0062] S2. Fill the sand box 11 with dry sand 12 and compact it. When the sand box 11 is compacted, cover the top surface of the sand box 11 with a film 13, and evacuate the sand box 11 to compact the dry sand 12 in the sand box 11. The vacuum degree in the sand box 11 is 0.01 MPa to 0.07 MPa.

[0063] S3. Install the pouring cup 21 on the top of the sand box 11, so that the pouring cup 21 is connected to the top of the runner foam model 22, and prepare for the introduction of the molten metal.

[0064] S4, pouring molten metal through the pouring cup 21, the molten metal sequentially melts the runner foam model 22 and the casting foam model 23, and combines with the solid insert 24 in the cavity formed by the casting foam model 23 and the dry sand 12.

[0065] S5. After the pouring is completed, when the bimetallic interface reaches 500°C, the power supply device 34 is started to apply a DC electric field to the solid insert 24 and the metal melt for a certain period of time until the bimetallic interface temperature is lower than 400°C and then the electric field is turned off.

[0066] S6. After the molten metal in the sand box 11 solidifies, the vacuum of the sand box 11 is released, the first electrode 31 and the second electrode 32 are removed, and the runner formed by the runner foam model 22 is removed, thereby obtaining a bimetallic casting.

[0067] In this embodiment, the power supply device 34 is a DC current-stabilized voltage-stabilized power supply or an electric pulse generator. The DC electric field applied to the solid insert 24 and the metal melt by the DC current-stabilized voltage-stabilized power supply has a current density of 300 to 500 A / cm 2 The pulse electric field applied to the solid inlay 103 and the melt by an electric pulse generator has a current density of 300 to 500 A / cm 2 , the frequency is 500Hz, and the current waveform is a bidirectional rectangular wave.

[0068] The following takes aluminum / magnesium bimetallic castings as an example to illustrate how to achieve the regulation of the interface bonding performance of aluminum / magnesium metal solid-liquid composite casting.

[0069] The casting foam model is designed as a cube of 35×35×100mm, and the solid insert is a cylinder with a diameter of 10mm and a height of 160mm. The material of the solid insert is A356 aluminum alloy, and the poured metal liquid is AZ91D magnesium alloy. The height of the solid insert extending out of the casting foam model part in the composite model assembly is 30mm.

[0070] During use, first put the composite model assembly into the sand box, and clamp the first electrode at the upper end of the solid insert extending out of the model, and embed the second electrode at the bottom of the connection between the casting foam model and the runner; the cable connects the two electrodes to the DC current-stabilized voltage-stabilized electric / electric pulse generator; vibrate the sand filling until the sand box is filled, and after the sand box is filled, cover the top with a layer of plastic film, and evacuate the sand box through a vacuum tube, with a vacuum degree of 0.03MPa; then install the pouring cup on the top of the runner foam model to complete the installation of the composite model assembly, and then pour the AZ91D magnesium alloy liquid from the pouring cup, with a pouring temperature of 735℃. 3-6min after the pouring is completed, when the temperature of the bimetallic interface is 500℃, a DC electric field is applied to the solid insert and the melt through a DC current-stabilized voltage-stabilized power supply, with a current density of 150A / cm 2 The electric field lasts for 7-9 minutes until the temperature of the bimetallic interface is lower than 400°C and then the electric field is turned off.

[0071] During the entire casting process, Figure 2 (a) shows the foam model and aluminum alloy assembly state before pouring. When the magnesium alloy melt contacts the foam, the foam decomposes rapidly under high heat capacity. Once the molten magnesium alloy contacts the A356 inlay, a thin chill zone is first formed, as shown in Figure 2. Figure 2 (b) At the same time, the element diffusion between the A356 inlay and the AZ91D melt continues in this process. Under the action of latent heat release and the high temperature of the magnesium melt, the surface melting of the aluminum inlay and the remelting of the quenching zone occur, as shown in Figure 2 (c) As shown. Due to the concentration gradient and solidification order, Al 3 Mg 2 , Al3 Mg 2 +Al 12 Mg 17 and Al 12 Mg 17 The intermetallic compound layers are formed sequentially, such as Figure 2 (d) to Figure 2 (f) is shown. Subsequently, Al 12 Mg 17 Preferential growth in the form of dendrites, such as Figure 2 Finally, due to the eutectic reaction, Al 12 Mg 17 +δ-Mg eutectic tissue area is formed, and the crystallization latent heat generated by the eutectic reaction makes α-Al 12 Mg 17 The dendrite root and dendrite arms are partially remelted, e.g. Figure 2 (h) As shown. Finally, the AZ91D magnesium alloy solidifies and the entire interface reaction layer is formed. In addition, due to the high Si content in the A356 alloy, Si atoms react with Mg atoms to form Mg 2 Si phase, due to Mg 2 The Si phase does not wet the Al-Mg intermetallic compound phase and cannot be captured by the solid-liquid interface during solidification, thus advancing to the magnesium alloy side. However, there is a thin oxide film remaining on the surface of the aluminum inlay between the eutectic structure area and the metal compound area, which hinders the mass transfer process and makes the Mg 2 Si phase gathers at the eutectic region boundary, such as Figure 2 (h) shown.

[0072] The DC electric field or pulse electric field applied by the present invention generates Joule heat at the bimetallic interface due to the Peltier effect, thereby reducing the influence of the vertical interface temperature gradient caused by the temperature difference on the solidification structure and preventing the Figure 2 (g) Coarse Al2O3 perpendicular to the interface 12 Mg 17 The formation of dendrites refines the structure. At the same time, the temperature field generated by Joule heat will also make Mg 2 The Si phase undergoes thermal migration and increases Figure 2 (d)~(g)Mg 2 The diffusion rate of Si phase in the interface. DC electric field can effectively reduce Figure 2 (g) Al grown vertically on the interface 12 Mg 17The distance between dendrites promotes the transformation of coarse dendrites to fine equiaxed crystals. In addition, the DC electric field will reduce the supercooling of the solidification process of the intermetallic compound, increase the nucleation rate, and have the effect of refining the structure. In addition, because electrons will collide with metal atoms under the action of high current density, the DC electric field can disturb the metal liquid through the momentum exchange between metal atoms and electrons, produce an undulating effect on the solidified structure, reduce the supercooling of the solidification process of the intermetallic compound, increase the nucleation rate, and achieve interface structure refinement. Thereby improving the mechanical properties of aluminum / magnesium bimetal.

[0073] Pulsed electric fields can achieve electromagnetic vibrations through the induced magnetic field generated by the electromagnetic effect. Figure 2 (b) When the magnesium melt contacts the aluminum inlay, the electromagnetic vibration can accelerate the breakage and melting of the oxide film on the surface of the aluminum inlay, and due to the unique flow effect of the pulse current, the current will Figure 2 In (g) and (h), the broken oxide film generates local high temperature, the oxide film at the interface is removed, and the mass transfer process during solidification is promoted, making Mg 2 The Si phase can diffuse into the eutectic region of the interface, greatly improving the uniformity of the structure of the bimetallic interface. Figure 2 (g) Al grown vertically on the interface 12 Mg 17 The dendrites are torn apart by the Lorentz force with constantly changing directions, generating a large number of new crystal nuclei. The disturbance of the induced magnetic field on the molten metal will cause the crystal nuclei to move in different directions, and finally a solidified structure with fine and uniform grains is obtained.

[0074] Implementation effect: The Al-Mg intermetallic compound at the magnesium / aluminum bimetallic interface is refined by more than 40%, the eutectic structure is refined by more than 30%, and the bonding strength of the bimetallic interface is increased by more than 35%.

[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A bimetallic solid-liquid composite casting molding device, characterized in that: The molding device comprises a sand box component (1), a composite model component (2) and an electric field generating device (3); The sand box assembly (1) comprises a sand box (11), dry sand (12) and a film (13); the dry sand (12) is filled in the sand box (11); and the sand box (11) is vacuumed so that the film (13) is tightly attached to the top surface of the sand box (11); The composite model assembly (2) comprises a pouring cup (21), a runner foam model (22), a casting foam model (23) and a solid insert (24); the runner foam model (22) is connected to the casting foam model (23) and both are arranged in dry sand (12); the pouring cup (21) is arranged on the top surface of the sand box (11) and is connected to the runner foam model (22); and the solid insert (24) is embedded in the casting foam model (23); The electric field generating device (3) comprises a first electrode (31), a second electrode (32), a cable (33) and a power supply device (34); the first electrode (31) is connected to one end of a solid insert (24); the second electrode (32) is embedded in a casting foam model (23) or a runner foam model (22); and the first electrode (31) and the second electrode (32) are respectively connected to the power supply device (34) via the cable (33).

2. The bimetallic solid-liquid composite casting molding device according to claim 1, characterized in that: The length of the solid insert (24) extending out of the casting foam model (23) is 10 mm to 30 mm.

3. The bimetallic solid-liquid composite casting molding device according to claim 2, characterized in that: The first electrode (31) and the second electrode (32) are both high temperature resistant graphite electrodes. The first electrode (31) is connected to the upper end of the solid insert (24) extending out of the casting foam model (23), and the first electrode (31) is connected to the positive electrode of the power supply device (34) through the cable (33). The second electrode (32) is embedded in the lower end of the casting foam model (23) or the lower end of the runner foam model (22), and the second electrode (32) is connected to the negative electrode of the power supply device (34) through the cable (33).

4. The bimetallic solid-liquid composite casting molding device according to claim 3, characterized in that: The runner foam model (22) is connected to the lower end of the casting foam model (23), and the second electrode (32) is embedded in the connection between the runner foam model (22) and the casting foam model (23).

5. The bimetallic solid-liquid composite casting molding device according to claim 1, characterized in that: The bottom surface of the sand box (11) is provided with a suction pipe (111) connected to an external negative pressure suction device.

6. The bimetallic solid-liquid composite casting molding device according to claim 1, characterized in that: The molding device also includes a vibration table (4), and the sand box (11) is fixedly arranged on the vibration table (4).

7. A bimetallic solid-liquid composite casting method, utilizing the bimetallic solid-liquid composite casting device as claimed in any one of claims 1 to 6, characterized in that: The steps include: S1, placing a casting foam model (23) and a runner foam model (22) connected as one body in a sand box (11), embedding a solid insert (24) in the casting foam model (23), installing a first electrode (31) at one end of the solid insert (24), inserting a second electrode (32) into the casting foam model (23) or the runner foam model (22), and connecting the first electrode (31) and the second electrode (32) to a power supply device (34) via a cable (33); S2, filling the sand box (11) with dry sand (12) and compacting it with vibration. When the sand box (11) is compacted, a film (13) is covered on the top surface of the sand box (11), and the sand box (11) is evacuated to compact the dry sand (12) in the sand box (11); S3, installing a pouring cup (21) on the top of the sand box (11), so that the pouring cup (21) is connected to the top of the runner foam model (22); S4, pouring molten metal through the pouring cup (21), the molten metal sequentially melts the runner foam model (22) and the casting foam model (23), and combines with the solid insert (24) in the cavity formed by the casting foam model (23) and the dry sand (12); S5. After the pouring is completed, when the temperature of the bimetallic interface reaches 500° C., the power supply device (34) is started to apply a DC electric field to the solid insert (24) and the metal melt for a certain period of time until the temperature of the bimetallic interface is lower than 400° C., and then the electric field is turned off; S6. After the molten metal in the sand box (11) solidifies, the vacuum of the sand box (11) is released, the first electrode (31) and the second electrode (32) are removed, and the runner formed by the runner foam model (22) is removed, thereby obtaining a bimetallic casting.

8. The bimetallic solid-liquid composite casting method according to claim 7, characterized in that: The current density applied by the power supply device (34) to the solid insert (24) and the metal melt is 300-500A / cm 2 .

9. The bimetallic solid-liquid composite casting method according to claim 7, characterized in that: The vacuum degree in the sand box (11) is 0.01 MPa to 0.07 MPa.

10. The bimetallic solid-liquid composite casting method according to claim 7, characterized in that: The power supply device (34) is a DC current-stabilized voltage-stabilized power supply or an electric pulse generator.

Citation Information

Patent Citations

  • Method for improving corrosion resistance of cast iron casting

    CN106424668A

  • Method for liquid-liquid compounding of aluminum / magnesium bimetal through lost foam casting and aluminum / magnesium bimetal

    CN113290231A

  • Ultrasonic-assisted lost foam casting device for magnesium-aluminum bimetal casting and application

    CN113333676A

  • Bimetal composite material preparation method based on electromagnetic liquid-solid forming

    CN113909457A

  • Equipment and method for magnetic field assisted lost foam casting of magnesium-aluminum bimetal casting

    CN116944472A