A method for recycling and reusing waste materials of wet-process sulfide electrolyte membrane

Through the wet sulfide electrolyte membrane waste recycling method, the problems of waste waste and battery short circuit in sulfide electrolyte membrane production are solved, and cost reduction and performance improvement are achieved.

CN118572239BActive Publication Date: 2024-11-26SHANGHAI FIRM LITHIUM NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411052893.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-26
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

Waste of waste generated during the production of sulfide electrolyte membrane leads to high costs, and the brittleness of the calendered sulfide electrolyte layer causes a short circuit in the battery, affecting the energy density.

Method used

The wet sulfide electrolyte membrane waste recycling method includes separation, grinding, filtration, drying, crushing and re-preparing slurry, combining adhesive and organic solvents, coating and rolling, and preparing sulfide electrolyte with high mechanical strength, preparation of sulfide electrolytes with high mechanical strength, including separation, grinding, filtration, drying, crushing, and re-preparing slurry, combining adhesive and organic solvents, coating and rolling. membrane.

Benefits of technology

The effective recycling of sulfide electrolyte membrane waste is achieved, the production cost is reduced, utilization is improved, and the conductivity and tensile strength of the electrolyte membrane are improved, avoiding battery short circuit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention discloses a method for recycling and reusing wet sulfide electrolyte membrane waste; comprising: S1, initial treatment of sulfide electrolyte membrane waste: first separating the sulfide electrolyte membrane waste from the substrate to obtain pure sulfide electrolyte membrane waste; S2, wet grinding the waste of S1 to obtain slurry A; S3, filtering, washing, drying and crushing the slurry obtained from S2 to obtain recycled powder; S4, mixing the powder obtained from S3 with an adhesive and an organic solvent to prepare slurry B; S5, coating the slurry B obtained from S4 on the substrate material, drying and peeling to obtain a sulfide electrolyte membrane. The present invention also discloses a sulfide electrolyte membrane prepared by the above method. The cost of sulfide electrolyte raw materials is high, and the method of the present invention has a simple process route, and the sulfide electrolyte waste is recycled, which reduces the production cost and improves the utilization rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer materials, and in particular to a method for recycling and reusing wet-process sulfide electrolyte membrane waste. Background Art

[0002] All-solid-state lithium batteries are believed to have high safety and energy density, providing new options for electric vehicles and energy storage devices. Among all solid electrolytes, sulfide electrolytes have ionic conductivity comparable to that of liquid electrolytes. Although sulfide solid electrolytes can be easily densified into films by dry calendering, the sulfide electrolyte membranes prepared by this process are generally thicker, and an excessively thick sulfide electrolyte layer will result in lower-than-expected battery-level energy density. In addition, the calendered sulfide solid electrolyte layer will break during the cycle due to its brittleness, causing the battery to short-circuit.

[0003] Inspired by the manufacturing of binder-assisted electrodes in traditional lithium-ion batteries, a polymer binder is combined with a sulfide solid electrolyte to prepare a thin sulfide solid electrolyte layer with high mechanical strength through a wet coating process. This wet coating process can be well integrated with the existing lithium-ion battery industry line and can be quickly introduced into the production line to achieve commercial production of solid-state lithium batteries.

[0004] However, the raw material cost of sulfide electrolyte is high and the synthesis cost is high. In the process of producing sulfide electrolyte membrane, the sulfide electrolyte is mixed with a binder to prepare a diaphragm. This process will produce some electrolyte membrane waste. The electrolyte membrane waste is composed of sulfide electrolyte and binder, and the binder accounts for between 0.5% and 10%. The generation of these electrolyte membrane wastes causes a lot of waste. For this reason, in the production process of sulfide electrolyte membrane, sulfide electrolyte waste should be recycled to reduce waste, reduce production costs, and improve utilization. Summary of the invention

[0005] The technical problem to be solved by the present invention is to reduce the waste of raw materials in the production process of sulfide electrolyte membranes, and provide a method for recycling and reusing wet sulfide electrolyte membrane waste. By separating the sulfide electrolyte from the binder, a recyclable sulfide electrolyte is obtained, and the membrane is re-made, the sulfide electrolyte membrane waste is recycled, and the cost reduction and efficiency improvement of sulfide batteries are achieved.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] <First aspect>

[0008] The present invention discloses a method for recycling and reusing waste materials of a wet-process sulfide electrolyte membrane, comprising the following steps:

[0009] S1. Initial treatment of sulfide electrolyte membrane waste recovery: firstly, the sulfide electrolyte membrane waste is separated from the substrate to obtain pure sulfide electrolyte membrane waste;

[0010] S2, wet grinding the waste material of S1 to obtain slurry A;

[0011] S3, filtering, washing, drying and crushing the slurry obtained in S2 to obtain a regenerated powder;

[0012] S4, mixing the recycled powder obtained in S3 with an adhesive and an organic solvent to prepare slurry B;

[0013] S5. Apply the slurry B prepared in S4 onto the base material, dry it, peel it off, and roll it to obtain a sulfide electrolyte membrane.

[0014] By initially treating wet sulfide electrolyte waste, wet grinding, filtering, drying, pulping and coating to obtain sulfide electrolyte membrane, the sulfide electrolyte membrane waste can be recycled, thereby achieving cost reduction and efficiency improvement of sulfide batteries.

[0015] As an embodiment of the present invention, the sulfide electrolyte membrane waste is a non-film-forming block waste or a cracked membrane sheet, and the sulfide electrolyte membrane waste is composed of a sulfide electrolyte and a binder, and the mass fraction of the binder in the electrolyte membrane waste is 0.5-10%.

[0016] Preferably, the sulfide electrolyte is LiPSCl, the binder is SBR (styrene-butadiene rubber), and the mass ratio of SBR in the sulfide electrolyte membrane waste is 1%-10%.

[0017] As an embodiment of the present invention, in step S1, the sulfide electrolyte membrane waste and the substrate are separated by a stripping reel or solvent immersion, and the solvent is at least one of n-heptane, xylene, n-hexane, and butyl butyrate.

[0018] As an embodiment of the present invention, the wet grinding in step S2 is to mix the waste material in S1 with a low-polarity solvent and grind it in a nano sand mill.

[0019] As an embodiment of the present invention, the wet grinding time in step S2 is 2 to 4 hours; the diameter of the zirconium ball during wet grinding is 0.1 mm to 2 mm, the circulation flow rate is 20 to 40 kg / h, and the rotation speed is 1000 to 10000 r / min. Avoid causing the grinding particles to be too large or wasting solvent.

[0020] Specifically, the low polarity solvent is one or a mixed solvent of n-hexane, n-heptane, xylene, butyl butyrate, etc. When the solvent is a polar solvent such as water or methanol, it will react with the electrolyte, causing the sulfide electrolyte to be deactivated; while low polarity solvents such as tetrahydrofuran, ethyl acetate, dimethyl ether, etc. will have a significant performance damage to the sulfide electrolyte.

[0021] As an embodiment of the present invention, the slurry A obtained by wet grinding in step S2 has a solid content of 10% to 65%.

[0022] As an embodiment of the present invention, in step S3, a low-polarity solvent is used to filter and wash the slurry A obtained in S2.

[0023] Specifically, the low polarity solvent is one or a mixed solvent of n-hexane, n-heptane, xylene, and butyl butyrate.

[0024] Specifically, the screening particle size during the filtration is 0.1-3 μm.

[0025] Specifically, the cleaning method is suction filtration and flushing or centrifugal washing.

[0026] As an embodiment of the present invention, the drying parameters in step S3 are: temperature 60-120° C., time 4-12 h.

[0027] As an embodiment of the present invention, the pulverizing method in step S3 is ball milling, high-speed pulverizer pulverization or air flow pulverizer pulverization.

[0028] Specifically, the rotation speed of the pulverization is 10000-18000 rpm, the pulverization is performed 3-6 times, and the time of each pulverization is 30-60 seconds, so as to obtain a regenerated powder with a particle size of 15-30 μm.

[0029] As an embodiment of the present invention, in step S4, the adhesive is one or more of styrene-butadiene rubber, nitrile rubber, and polyvinylidene fluoride. In the process of grinding and recycling, there is a risk of demulsification of the adhesive, resulting in high viscosity of the slurry, or easy powdering and rigidification of the membrane when forming the film again, so a new adhesive needs to be used to make the film.

[0030] As an embodiment of the present invention, the organic solvent in step S4 is a low polarity solvent.

[0031] Specifically, the low polarity solvent is one or a mixed solvent of n-hexane, n-heptane, xylene, and butyl butyrate.

[0032] As an embodiment of the present invention, when the recycled powder obtained in S3 is mixed with an adhesive and an organic solvent in step S4, the adhesive accounts for 0.5% to 10% of the total mass of the recycled powder and the adhesive; and the solid content of the slurry B is 15 to 60%.

[0033] As an embodiment of the present invention, the substrate material in step S5 is a release film, a PTFE film or a PET film.

[0034] As an embodiment of the present invention, the roller pressing pressure in step S5 is 200-1000 MPa.

[0035] As an embodiment of the present invention, the drying temperature in step S5 is 50-120°C.

[0036] <Second Aspect>

[0037] The present invention also provides a sulfide electrolyte membrane prepared by any of the above-mentioned methods for recycling and reusing wet-process sulfide electrolyte membrane waste.

[0038] As an embodiment of the present invention, the thickness of the sulfide electrolyte membrane is 30-50 μm.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] 1) The present invention utilizes the sulfide electrolyte edge waste, performs wet grinding, filtering, drying, pulping, coating and other process steps, and realizes the recycling of sulfide electrolyte membrane waste;

[0041] 2) The wet process effectively removes impurities such as binders in the waste, and the regenerated sulfide electrolyte powder prepared is of high purity; and through high-speed crushing and roller pressing processes, the sulfide electrolyte waste can be refined, which is conducive to the effect of re-film formation;

[0042] 3) The preparation process of the present invention is simple and can be combined with the existing coating machine production line, with low transformation cost, which is more conducive to industrialization;

[0043] 4) The method of the present invention is used to recycle and reuse sulfide electrolyte membrane waste, and the obtained recycled electrolyte membrane has good electrical conductivity and tensile strength. DETAILED DESCRIPTION

[0044] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0045] Example 1

[0046] A method for recycling and reusing wet-process sulfide electrolyte membrane waste comprises the following steps:

[0047] (1) Initial treatment of sulfide electrolyte membrane waste recycling: first separate the sulfide electrolyte membrane waste from the substrate to obtain pure sulfide electrolyte membrane waste;

[0048] The sulfide electrolyte membrane waste refers to non-film-forming block waste or cracked membrane sheets, which are composed of sulfide electrolyte LiPSCl and binder SBR (the mass ratio of the two is 97:3), and the separation method adopted is solution immersion separation; the solvent used is xylene, and the substrate is PET film.

[0049] (2) The waste material of step (1) was placed in a nano sand mill and ground for 2 h. The diameter of the zirconium ball for wet grinding was 0.5 mm, the circulation flow rate was 20 kg / h, the rotation speed was 3000 r / min, and the solvent used was xylene to obtain slurry A with a solid content of 30%;

[0050] (3) The slurry A obtained in step (2) was filtered and washed three times with xylene solvent, and vacuum dried at 60°C for 12 h; then crushed in a high-speed crusher at a speed of 10,000 rpm for 3 times, each time for 40 s, to obtain a regenerated powder with a particle size of about 30 μm;

[0051] (4) mixing the powder obtained in step (3) with styrene-butadiene rubber and xylene, and stirring for 12 h to prepare slurry B, wherein the styrene-butadiene rubber accounts for 1% of the solid mass and the solid content of slurry B is 40%;

[0052] (5) The slurry B prepared in step (4) is coated on a release film material through a coating machine, dried at 80° C., peeled off, and rolled at a rolling pressure of 300 MPa to obtain a sulfide electrolyte membrane with a thickness of 30 μm.

[0053] Example 2

[0054] A method for recycling and reusing wet-process sulfide electrolyte membrane waste comprises the following steps:

[0055] (1) Initial treatment of sulfide electrolyte membrane waste recycling: first separate the sulfide electrolyte membrane waste from the substrate to obtain pure sulfide electrolyte membrane waste;

[0056] The sulfide electrolyte membrane waste refers to the block waste or cracked membrane that does not form a membrane, which is composed of sulfide electrolyte LiPSCl and binder SBR (the mass ratio of the two is 94:6). The separation method adopted is solution immersion separation, the solvent used is xylene, and the substrate is a release film.

[0057] (2) The waste material of step (1) was placed in a nano sand mill and ground for 4 hours. The diameter of the zirconium ball for wet grinding was 0.5 mm, the circulation flow rate was 30 kg / h, the rotation speed was 4000 r / min, and the solvent used was n-hexane to obtain slurry A with a solid content of 35%;

[0058] (3) The slurry A obtained in step (2) was filtered and washed three times with xylene solvent, vacuum dried at 60°C for 12 h, and then crushed in a high-speed crusher at a speed of 13,000 rpm for 3 times, each time for 30 s, to obtain a regenerated powder with a particle size of about 30 μm;

[0059] (4) mixing the powder obtained in step (3) with styrene-butadiene rubber and a xylene / n-hexane mixed solvent (the volume ratio of the mixed solvent is 1:1), wherein the styrene-butadiene rubber accounts for 1.5% of the solid mass ratio, and stirring for 12 h to prepare slurry B, wherein the solid content of slurry B is 40%;

[0060] (5) The slurry B prepared in step (4) is coated on a release film substrate by a coating machine, dried at 80° C., peeled off, and rolled at a rolling pressure of 300 MPa to obtain a sulfide electrolyte membrane with a thickness of 30 μm.

[0061] Example 3

[0062] A method for recycling and reusing wet-process sulfide electrolyte membrane waste comprises the following steps:

[0063] (1) Initial treatment of sulfide electrolyte membrane waste recycling: First, the sulfide electrolyte membrane waste is separated from the substrate to obtain pure sulfide electrolyte membrane waste; the sulfide electrolyte membrane waste refers to non-film-forming block waste or cracked membrane sheets, which are composed of sulfide electrolyte LiPSCl and binder SBR (the mass ratio of the two is 98:2). The separation method used is roll-to-roll peeling, and the substrate is a release film.

[0064] (2) The waste material of step (1) was placed in a nano sand mill and ground for 2 h. The diameter of the zirconium ball for wet grinding was 0.5 mm, the circulation flow rate was 35 kg / h, the rotation speed was 3200 r / min, and the solvent used was butyl butyrate to obtain slurry A with a solid content of 30%;

[0065] (3) The slurry A obtained in step (2) was filtered and washed three times with butyl butyrate solvent, vacuum dried at 60°C for 12 h, and then crushed in a high-speed crusher at a speed of 15,000 rpm for 4 times, each time for 60 s, to obtain a regenerated powder with a particle size of about 20 μm;

[0066] (4) mixing the powder obtained in step (3) with styrene-butadiene rubber and butyl butyrate, with the styrene-butadiene rubber accounting for 2% of the solid mass ratio, and stirring for 12 h to prepare slurry B with a solid content of 50%;

[0067] (5) The slurry B prepared in step (4) is coated on a release film substrate by a coating machine, dried at 80° C., peeled off, and rolled at a rolling pressure of 250 MPa to obtain a sulfide electrolyte membrane with a thickness of 50 μm.

[0068] Example 4

[0069] A method for recycling and reusing wet-process sulfide electrolyte membrane waste comprises the following steps:

[0070] (1) Initial treatment of sulfide electrolyte membrane waste recycling: first separate the sulfide electrolyte membrane waste from the substrate to obtain pure sulfide electrolyte membrane waste;

[0071] The sulfide electrolyte membrane waste refers to the block waste or cracked membrane that does not form a membrane, which is composed of sulfide electrolyte LiPSCl and binder SBR (the mass ratio of the two is 97:3). The separation method adopted is roll-to-roll peeling, and the substrate is a release film.

[0072] (2) The waste material of step (1) was placed in a nano sand mill and ground for 3 hours. The diameter of the zirconium ball for wet grinding was 0.2 mm, the circulation flow rate was 25 kg / h, the rotation speed was 3500 r / min, and the solvent used was xylene to obtain slurry A with a solid content of 30%;

[0073] (3) The slurry A obtained in step (2) was filtered and washed three times with xylene solvent, vacuum dried at 60°C for 12 h, and then crushed in a high-speed crusher at a speed of 18,000 rpm for 6 times, each time for 30 s, to obtain a regenerated powder with a particle size of about 15 μm;

[0074] (4) The powder obtained in step (3) was mixed with nitrile rubber and xylene, with the styrene-butadiene rubber accounting for 3% of the solid mass ratio, and stirred for 12 h to prepare slurry B with a solid content of 50%;

[0075] (5) The slurry B prepared in step (4) is coated on a release film material through a coating machine, dried at 80° C., peeled off, and rolled at a rolling pressure of 350 MPa to obtain a sulfide electrolyte membrane with a thickness of about 50 μm.

[0076] Example 5

[0077] A method for recycling and reusing wet-process sulfide electrolyte membrane waste comprises the following steps:

[0078] (1) Initial treatment of sulfide electrolyte membrane waste recycling: First, the sulfide electrolyte membrane waste is separated from the substrate to obtain pure sulfide electrolyte membrane waste; the sulfide electrolyte membrane waste refers to non-film-forming block waste or cracked membrane sheets, which are composed of sulfide electrolyte LiPSCl and binder SBR (the mass ratio of the two is 97:3). The separation method used is roll-to-roll peeling, and the substrate is a release film.

[0079] (2) The waste material of step (1) was placed in a nano sand mill and ground for 3 h. The diameter of the zirconium ball for wet grinding was 0.2 mm, the circulation flow rate was 25 kg / h, the rotation speed was 3500 r / min, and the solvent used was n-heptane to obtain slurry A with a solid content of 30%;

[0080] (3) The slurry A obtained in step (2) was filtered and washed three times with n-heptane solvent, vacuum dried at 60°C for 12 h, and then crushed in a high-speed crusher at a speed of 18,000 rpm for 6 times, each time for 30 s, to obtain a regenerated powder with a particle size of about 15 μm;

[0081] (4) The powder obtained in step (3) was mixed with nitrile rubber and n-heptane, with the styrene-butadiene rubber accounting for 3% of the solid mass ratio, and stirred for 12 h to prepare slurry B with a solid content of 50%;

[0082] (5) The slurry B prepared in step (4) is coated on a release film material through a coating machine, dried at 80° C., peeled off, and rolled at a rolling pressure of 350 MPa to obtain a sulfide electrolyte membrane with a thickness of about 50 μm.

[0083] Comparative Example 1

[0084] This comparative example is the original membrane of the sulfide electrolyte membrane waste.

[0085] Comparative Example 2

[0086] A method for recycling and reusing wet-process sulfide electrolyte membrane waste comprises the following steps:

[0087] (1) Initial treatment of sulfide electrolyte membrane waste recycling: first separate the sulfide electrolyte membrane waste from the substrate to obtain pure sulfide electrolyte membrane waste;

[0088] The sulfide electrolyte membrane waste refers to the block waste or cracked membrane that does not form a membrane, which is composed of sulfide electrolyte LiPSCl and binder SBR (the mass ratio of the two is 97:3). The separation method used is solution immersion separation, the solution used is dimethyl ether, and the substrate is PET film.

[0089] (2) The waste material of step (1) was placed in a nano sand mill and ground for 3 h. The diameter of the zirconium ball for wet grinding was 0.2 mm, the circulation flow rate was 25 kg / h, the rotation speed was 3500 r / min, and the solvent used was dimethyl ether + xylene (the volume ratio of the mixed solvent was 1:2), to obtain slurry A with a solid content of 30%;

[0090] (3) The slurry A obtained in step (2) was filtered and washed three times with xylene solvent, vacuum dried at 60°C for 12 h, and then crushed in a high-speed crusher at a speed of 18,000 rpm for 6 times, each time for 30 s, to obtain a regenerated powder with a particle size of about 15 μm;

[0091] (4) mixing the powder obtained in step (3) with nitrile rubber and xylene, with the styrene-butadiene rubber accounting for 3% of the solid mass ratio, and stirring for 12 hours to prepare slurry B with a solid content of 50%;

[0092] (5) The slurry B prepared in step (4) is coated on a release film material through a coating machine, dried at 80° C., peeled off, and rolled at a rolling pressure of 350 MPa to obtain a sulfide electrolyte membrane with a thickness of about 50 μm.

[0093] Comparative Example 3

[0094] A method for recycling and reusing wet-process sulfide electrolyte membrane waste comprises the following steps:

[0095] (1) Initial treatment of sulfide electrolyte membrane waste recycling: first separate the sulfide electrolyte membrane waste from the substrate to obtain pure sulfide electrolyte membrane waste;

[0096] The sulfide electrolyte membrane waste refers to the block waste or cracked membrane that does not form a membrane, which is composed of sulfide electrolyte LiPSCl and binder SBR (the mass ratio of the two is 96:4). The separation method adopted is solution immersion separation, the solution used is n-butyl ether, and the substrate is PET film.

[0097] (2) The waste material of step (1) was placed in a nano sand mill and ground for 3 h. The diameter of the zirconium ball for wet grinding was 0.2 mm, the circulation flow rate was 25 kg / h, the rotation speed was 3500 r / min, and the solvent used was n-butyl ether to obtain slurry A with a solid content of 30%;

[0098] (3) The slurry A obtained in step (2) was filtered and washed three times with n-butyl ether solvent, vacuum dried at 60°C for 12 h, and then crushed in a high-speed crusher at a speed of 18,000 rpm for 6 times, each time for 30 s, to obtain a regenerated powder with a particle size of about 15 μm;

[0099] (4) mixing the powder obtained in step (3) with nitrile rubber and n-butyl ether, with styrene-butadiene rubber accounting for 3% of the solid mass ratio, and stirring for 12 h to prepare slurry B with a solid content of 50%;

[0100] (5) The slurry B prepared in step (4) is coated on a release film material through a coating machine, dried at 80° C., peeled off, and rolled at a rolling pressure of 350 MPa to obtain a sulfide electrolyte membrane with a thickness of about 50 μm.

[0101] Comparative Example 4

[0102] A method for recycling and reusing wet-process sulfide electrolyte membrane waste comprises the following steps:

[0103] (1) Initial treatment of sulfide electrolyte membrane waste recycling: first separate the sulfide electrolyte membrane waste from the substrate to obtain pure sulfide electrolyte membrane waste;

[0104] The sulfide electrolyte membrane waste refers to the block waste or cracked membrane that does not form a membrane, which is composed of sulfide electrolyte LiPSCl and binder SBR (mass ratio is 97:3). The separation method adopted is solution immersion separation, the solution used is n-butyl ether, and the substrate is PET film.

[0105] (2) The waste material of step (1) was placed in a nano sand mill and ground for 3 h. The diameter of the zirconium ball for wet grinding was 0.2 mm, the circulation flow rate was 25 kg / h, the rotation speed was 3500 r / min, and the solvent used was n-butyl ether / n-heptane (the volume ratio of the mixed solvent was 2:1), to obtain slurry A with a solid content of 30%;

[0106] (3) The slurry A obtained in step (2) was filtered and washed three times with a mixed solvent of n-butyl ether / n-heptane, vacuum dried at 60°C for 12 h, and then crushed in a high-speed crusher at a speed of 18,000 rpm for 6 times, each time for 30 s, to obtain a regenerated powder with a particle size of about 15 μm;

[0107] (4) The powder obtained in step (3) was mixed with nitrile rubber and a mixed solvent of n-butyl ether / n-heptane, with the styrene-butadiene rubber accounting for 3% of the solid mass ratio, and stirred for 12 hours to prepare slurry B with a solid content of 50%;

[0108] (5) The slurry B prepared in step (4) is coated on a release film material through a coating machine, dried at 80° C., peeled off, and rolled at a rolling pressure of 350 MPa to obtain a sulfide electrolyte membrane with a thickness of about 50 μm.

[0109] Effect Example

[0110] In order to evaluate the ionic conductivity of the regenerated sulfide electrolyte membrane, the electrolyte membrane was made into a sheet, placed in an all-solid-state battery mold, and matched with blocking electrodes at both ends for analysis using the AC impedance method.

[0111] The calculation formula is as follows:

[0112] σLi+=L / (RS)

[0113] Where, σLi+——ionic conductivity of solid electrolyte (ms / cm);

[0114] L——solid electrolyte thickness (cm);

[0115] R——intrinsic resistance of solid electrolyte (Ω);

[0116] S——Cross-sectional area of ​​solid electrolyte (cm 2 );

[0117] The results of testing the sulfide electrolyte membranes in Examples 1 to 5 and Comparative Examples 1 to 4 according to the above method are shown in Table 1.

[0118] Table 1 Test results of electrolyte membranes of various embodiments and comparative examples

[0119]

[0120] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A method for recycling and reusing waste wet-process sulfide electrolyte membranes, characterized in that: The following steps are involved: S1. Initial treatment of sulfide electrolyte membrane waste recycling: Use a stripping and reeling machine or solvent immersion to separate the sulfide electrolyte membrane waste from the substrate to obtain pure sulfide electrolyte membrane waste; S2, mixing the waste material obtained in S1 with a low-polarity solvent, and performing wet grinding to obtain slurry A; S3, filtering, washing, drying and crushing the slurry obtained in S2 with a low-polarity solvent to obtain a regenerated powder; S4, mixing the recycled powder obtained in S3 with an adhesive and an organic solvent to prepare slurry B; the organic solvent is a low-polarity solvent; S5, coating the slurry B prepared in S4 on a base material, drying, peeling, and rolling to obtain a sulfide electrolyte membrane; The low polarity solvent is one or a mixed solvent of n-hexane, n-heptane, xylene, and butyl butyrate; The sulfide electrolyte membrane waste is composed of a sulfide electrolyte and a binder, wherein the mass fraction of the binder in the electrolyte membrane waste is 0.5-10%; and the sulfide electrolyte is LiPSCl.

2. The method according to claim 1, characterized in that The binder is styrene-butadiene rubber; the mass proportion of the styrene-butadiene rubber in the sulfide electrolyte membrane waste is 1% to 10%.

3. The method according to claim 1, characterized in that In step S1, the solvent is one or more of n-heptane, xylene, n-hexane, and butyl butyrate.

4. The method according to claim 1, characterized in that: The wet grinding in step S2 is performed in a nano sand mill; the diameter of the zirconium balls during the wet grinding is 0.1 mm to 2 mm, the circulation flow rate is 20 to 40 kg / h, the rotation speed is 1000 to 10000 r / min, and the grinding time is 2 to 4 hours.

5. The method according to claim 1, characterized in that The slurry A obtained by wet grinding in step S2 has a solid content of 10% to 65%.

6. The method according to claim 1, characterized in that The sieve particle size during filtration in step S3 is 0.1-3 μm; the cleaning method is suction filtration or centrifugal washing; The drying parameters in step S3 are: temperature 60-120° C., time 4-12 hours; and pulverization method is ball milling, high-speed pulverizer or air flow pulverizer.

7. The method according to claim 1, characterized in that The adhesive in step S4 is one or more of styrene-butadiene rubber, nitrile rubber, and polyvinylidene fluoride; the adhesive accounts for 0.5% to 10% of the total mass of the recycled powder and the adhesive; and the solid content of the slurry B is 15 to 60%.

8. The method according to claim 1, characterized in that The base material in step S5 is a release film, a PTFE film or a PET film; the drying temperature is 50-120° C.; and the rolling pressure is 200-1000 MPa.

9. A sulfide electrolyte membrane, characterized in that: The invention is prepared by the method for recycling and reusing wet sulfide electrolyte membrane waste as described in any one of claims 1 to 8.