Composite positive electrode material, positive electrode sheet containing the same, and solid-state lithium-ion battery
By using MOF and metal oxide to coat the cathode material in solid-state lithium-ion batteries, the performance problem of matching the sulfide solid electrolyte with the high-voltage cathode is solved, excellent discharge specific capacity and cycle performance are achieved, and the battery's performance is improved. Security.
Patent Information
- Application Number
- CN202411061081.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Sulfide solid electrolytes cannot achieve both excellent discharge specific capacity and cycle performance when matched with high-voltage cathodes, and are prone to react with trace amounts of water, leading to decomposition and the generation of flammable and toxic gases, affecting battery safety.
Composite cathode materials are used, and the first and second cathode material particles are coated with MOF materials and metal oxides, combined with sulfide solid electrolytes to avoid side reactions and water decomposition and ensure high ionic conductivity.
It achieves excellent discharge specific capacity and cycle performance when solid-state lithium-ion batteries use NCM811 cathode material, while improving the safety and stability of the battery.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a composite positive electrode material, a positive electrode sheet containing the same and a solid-state lithium ion battery. Background Art
[0002] Traditional lithium-ion batteries have safety issues due to the presence of flammable organic liquid electrolytes. Solid-state batteries can provide higher energy density and better safety. Inorganic solid electrolytes have high thermal stability and ionic conductivity. Inorganic solid electrolytes include oxide solid electrolytes, sulfide solid electrolytes and halide solid electrolytes, among which sulfide solid electrolytes have the highest ionic conductivity.
[0003] However, sulfide solid electrolytes have some disadvantages, such as low oxidation potential (2.5 V vs. Li / Li+). When they are matched with high-voltage positive electrodes, side reactions will occur, resulting in increased interfacial impedance and reduced electrochemical performance. This phenomenon has become one of the key scientific issues that hinder the commercialization of solid-state batteries based on sulfide solid electrolytes. In addition, it is very easy to react with trace water, which causes the sulfide solid electrolyte to decompose and generate hydrogen sulfide gas, which greatly reduces the ionic conductivity of the sulfide solid electrolyte, making it impossible to take into account both excellent discharge specific capacity and cycle performance. At the same time, hydrogen sulfide gas is a recognized flammable and toxic gas. Therefore, humidity control becomes crucial in the manufacturing process. Summary of the invention
[0004] In order to solve the problem that the solid electrolyte based on solid-state batteries in the prior art cannot take into account both excellent discharge capacity and cycle performance when matched with a high-voltage positive electrode, the present invention provides a composite positive electrode material and a positive electrode sheet and a solid-state lithium-ion battery containing the same. The composite positive electrode material matches the solid electrolyte, which can ensure the high ion conductivity of the solid electrolyte, and the resulting solid-state lithium-ion battery (especially when NCM811 is used as the positive electrode material) has excellent discharge capacity and cycle performance.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions.
[0006] In a first aspect, the present invention provides a composite positive electrode material, which includes positive electrode material particles and solid electrolyte particles;
[0007] The positive electrode material particles include a first positive electrode material particle and a second positive electrode material particle; the first positive electrode material particle includes a first positive electrode material core and a first coating layer; the second positive electrode material particle includes a second positive electrode material core and a second coating layer;
[0008] Wherein, the first coating layer comprises MOF material; the second coating layer comprises metal oxide;
[0009] The particle size of the core of the first positive electrode material is larger than that of the core of the second positive electrode material; and the particle size of the core of the second positive electrode material is larger than that of the solid electrolyte particles.
[0010] In a second aspect, the present invention provides a positive electrode sheet comprising the composite positive electrode material as described above.
[0011] In a third aspect, the present invention provides a solid-state lithium-ion battery, which includes a positive electrode sheet, a solid electrolyte layer and a negative electrode sheet as described above.
[0012] The positive and progressive effects of the present invention are:
[0013] The present invention provides a composite positive electrode material. By respectively coating a first positive electrode material particle and a second positive electrode material particle with an MOF material and a metal oxide, when a solid-state lithium-ion battery is prepared with a solid electrolyte layer, side reactions between the solid electrolyte and the positive electrode material can be avoided, and adverse effects of trace water on the solid electrolyte can be avoided, thereby ensuring high ionic conductivity of the solid electrolyte. The obtained solid-state lithium-ion battery (especially when NCM811 is used as the positive electrode material) can have both excellent discharge specific capacity and cycle performance. DETAILED DESCRIPTION
[0014] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0015] Composite cathode materials
[0016] In the composite positive electrode material provided in the first aspect of the present invention, it comprises positive electrode material particles and solid electrolyte particles;
[0017] The positive electrode material particles include a first positive electrode material particle and a second positive electrode material particle; the first positive electrode material particle includes a first positive electrode material core and a first coating layer; the second positive electrode material particle includes a second positive electrode material core and a second coating layer;
[0018] Wherein, the first coating layer comprises MOF material; the second coating layer comprises metal oxide;
[0019] The particle size of the core of the first positive electrode material is larger than that of the core of the second positive electrode material; and the particle size of the core of the second positive electrode material is larger than that of the solid electrolyte particles.
[0020] In some optional embodiments, the thickness of the first coating layer is 10 nm-50 nm, for example, 20 nm or 30 nm.
[0021] In some optional embodiments, the thickness of the second coating layer is 2 nm-20 nm, for example, 10 nm.
[0022] In some optional embodiments, the Dv50 of the core of the first positive electrode material is 8μm-20μm, for example, 10.4μm or 15μm; the Dv50 of the core of the second positive electrode material is 2μm-5μm, for example, 3.3μm; the Dv50 of the solid electrolyte particles is 0.6μm-1.5μm, for example, 1.1μm or 1.3μm.
[0023] In some optional embodiments, the solid electrolyte particles satisfy: 1.7<Dv90 / Dv10<1.9; 1μm<Dv90<1.5μm; 0.6μm<Dv10<0.8μm.
[0024] In some optional embodiments, the content of the first positive electrode material particles is 30%-90%, for example, 34.8%, 45%, 49.8%, 55%, 62.7% or 67.5%, the content of the second positive electrode material particles is 5%-40%, for example, 7.5%, 12.7%, 18.1%, 20%, 22.8% or 30%, the content of the solid electrolyte particles is 5%-50%, for example, 9.5%, 20%, 27.1% or 47.5%, and the percentage is the mass percentage of each component in the composite positive electrode material.
[0025] In some optional embodiments, the mass ratio of the first positive electrode material particles to the second positive electrode material particles is (1-9):1, for example, 1.5:1 or 2.75:1.
[0026] In some optional embodiments, the mass ratio of the positive electrode material particles to the solid electrolyte particles is (1-9):1, for example, 2.5:1 or 3.75:1.
[0027] In some specific embodiments, in the composite positive electrode material, the mass ratio of the first positive electrode material particles to the second positive electrode material particles is 1.5:1, 2.75:1 or 9:1, and the mass ratio of the positive electrode material particles to the solid electrolyte particles is 3.75:1.
[0028] In some specific embodiments, in the composite positive electrode material, the mass ratio of the first positive electrode material particles to the second positive electrode material particles is 2.75:1, and the mass ratio of the positive electrode material particles to the solid electrolyte particles is 1:1, 2.5:1, 3.75:1 or 9:1.
[0029] In some optional embodiments, the MOF material includes one or both of a zirconium-based MOF material and a chromium-based MOF material.
[0030] In some preferred embodiments, the MOF material includes one or more of MOF-808, MOF-801, UiO-66 and MIL-101.
[0031] In some embodiments, the method for preparing the first positive electrode material particles comprises the following steps:
[0032] The mixed solution of the metal salt solution and the first positive electrode material core is mixed with the organic ligand solution, and the mixture is filtered and washed to obtain the product.
[0033] In some specific embodiments, the mixing temperature is 120° C., and the mixing time is 72 h.
[0034] In some specific embodiments, the metal salt solution is an acetic acid solution of zirconium chloride, and the organic ligand solution is a trimesic acid solution formed by dissolving trimesic acid in N,N-dimethylformamide.
[0035] In some specific embodiments, the metal salt solution is an acetic acid solution of zirconium oxychloride octahydrate, and the organic ligand solution is a fumaric acid solution formed by dissolving fumaric acid in N,N-dimethylformamide.
[0036] In some optional embodiments, the metal oxide includes one or more of zinc oxide, tin oxide, titanium oxide, copper oxide, tungsten oxide, zirconium oxide, aluminum oxide and niobium oxide.
[0037] In some optional embodiments, the first positive electrode material core and the second positive electrode material core each independently include one or more of lithium nickel cobalt manganese oxide, lithium nickel manganese oxide, lithium iron phosphate, lithium manganese iron phosphate and lithium cobalt oxide.
[0038] In a preferred embodiment, the core of the first positive electrode material is lithium nickel cobalt manganese oxide, for example, LiNi 0.8 Co 0.1 Mn 0.1 O2 or LiNi 0.6 Co 0.2 Mn 0.2 O2; the core of the second positive electrode material is lithium nickel cobalt manganese oxide, such as LiNi 0.8 Co 0.1 Mn 0.1 O2 or LiNi 0.6 Co 0.2 Mn 0.2 O2.
[0039] In a preferred embodiment, the core of the first positive electrode material is lithium nickel manganese oxide, for example, LiNi 0.5 Mn 1.5 O4; the core of the second positive electrode material is lithium nickel manganese oxide, such as LiNi0.5 Mn 1.5 O4.
[0040] In some specific embodiments, in the composite positive electrode material, the first positive electrode material particle includes a first positive electrode material core and a first coating layer; the second positive electrode material particle includes a second positive electrode material core and a second coating layer; wherein the first positive electrode material core and the second positive electrode material core are LiNi 0.8 Co 0.1 Mn 0.1 O2, the first coating layer is MOF-808, the second coating layer is ZrO2, the thickness of the first coating layer is, for example, 10nm, 20nm, 30nm or 50nm, and the thickness of the second coating layer is, for example, 2nm, 10nm or 20nm.
[0041] In some specific embodiments, in the composite positive electrode material, the first positive electrode material particle includes a first positive electrode material core and a first coating layer; the second positive electrode material particle includes a second positive electrode material core and a second coating layer; wherein the first positive electrode material core and the second positive electrode material core are LiNi 0.8 Co 0.1 Mn 0.1 O2, the first coating layer is MOF-801, the second coating layer is ZrO2, the thickness of the first coating layer is, for example, 30 nm, and the thickness of the second coating layer is, for example, 10 nm.
[0042] In some specific embodiments, in the composite positive electrode material, the first positive electrode material particle includes a first positive electrode material core and a first coating layer; the second positive electrode material particle includes a second positive electrode material core and a second coating layer; wherein the first positive electrode material core and the second positive electrode material core are LiNi 0.8 Co 0.1 Mn 0.1 O2, the first coating layer is MOF-808, the second coating layer is Nb2O5, the thickness of the first coating layer is, for example, 30 nm, and the thickness of the second coating layer is, for example, 10 nm.
[0043] In some specific embodiments, in the composite positive electrode material, the first positive electrode material particle includes a first positive electrode material core and a first coating layer; the second positive electrode material particle includes a second positive electrode material core and a second coating layer; wherein the first positive electrode material core and the second positive electrode material core are LiNi 0.5 Mn 1.5 O4, the first coating layer is MOF-808, the second coating layer is ZrO2, the thickness of the first coating layer is, for example, 30 nm, and the thickness of the second coating layer is, for example, 10 nm.
[0044] In some specific embodiments, in the composite positive electrode material, the first positive electrode material particle includes a first positive electrode material core and a first coating layer; the second positive electrode material particle includes a second positive electrode material core and a second coating layer; wherein the first positive electrode material core and the second positive electrode material core are LiNi 0.6 Co 0.2 Mn 0.2 O2, the first coating layer is MOF-808, the second coating layer is ZrO2, the thickness of the first coating layer is, for example, 30 nm, and the thickness of the second coating layer is, for example, 10 nm.
[0045] In some optional embodiments, the solid electrolyte particles are sulfide solid electrolyte particles, and the sulfide solid electrolyte particles include Li 10 GeP2S 12 、Li7P3S 11 , Li6PS5Cl, Li6PS5Br and Li6PS5I.
[0046] In some optional embodiments, the composite positive electrode material also includes a conductive agent, which includes one or more of graphite, graphene, carbon black, carbon fiber and carbon nanotubes; the content of the conductive agent is 1%-5%, for example, 4%, where the percentage is the mass percentage of the composite positive electrode material.
[0047] In a preferred embodiment, the conductive agent is carbon black and carbon fiber; the mass ratio of the carbon black to the carbon fiber is 1:(0.2-1.5), for example, 1:1.
[0048] In a specific embodiment, the carbon black is conductive carbon black SP (Super P).
[0049] In a specific embodiment, the carbon fiber includes one or more of carbon nanofiber (CNF), vapor grown carbon fiber (VGCF) and vapor grown carbon nanofiber (VGCNF).
[0050] In a specific embodiment, the conductive agent is conductive carbon black SP and vapor-grown carbon fiber; the mass ratio of the conductive carbon black SP to the vapor-grown carbon fiber is, for example, 1:1.
[0051] In some optional embodiments, the composite positive electrode material also includes a binder, and the binder includes one or more of polytetrafluoroethylene, styrene-butadiene rubber, ethylene-tetrafluoroethylene copolymer and ethylene trifluorochloroethylene copolymer; the content of the binder is 0.1%-2%, for example, 1%, and the percentage is the mass percentage of the composite positive electrode material.
[0052] In a specific embodiment, the binder is polytetrafluoroethylene (PTFE).
[0053] In some optional embodiments, the method for preparing the composite positive electrode material comprises the following steps:
[0054] The mixed material is ball-milled in a glove box to obtain a mass-shaped mixed material, and the mass-shaped mixed material is roll-pressed to obtain the mixed material; the mixed material includes the first positive electrode material particles, the second positive electrode material particles and the solid electrolyte particles.
[0055] In some preferred embodiments, the atmosphere of the glove box is argon.
[0056] In some preferred embodiments, the dew point temperature of the glove box is -80°C to -40°C, for example -60°C.
[0057] In some preferred embodiments, the rotation speed of the ball milling treatment is 100-1000 rpm, for example, 500 rpm; the time of the ball milling treatment is 0.5-3 h, for example, 2 h; the diameter of the zirconium beads for the ball milling treatment is 5 mm-20 mm, for example, 10 mm; the ball-to-material ratio of the ball milling treatment is (20-50):1, for example, 30:1.
[0058] In some preferred embodiments, the preset temperature of the roller pressing is 60-150°C, for example 80°C.
[0059] In some preferred embodiments, the roller pressing is performed until the surface capacity of the mass mixture is 1-10 mAh·cm -2 , for example, 2 mAh·cm -2 .
[0060] In a specific embodiment, the method for preparing the composite positive electrode material comprises the following steps:
[0061] The first positive electrode material particles, the second positive electrode material particles, Li6PS5Cl, Super P, VGCF and PTFE are mixed in a glove box to form a mixture; the mixture is ball-milled to obtain a mass mixture, and the mass mixture is roll-pressed to obtain; wherein the rotation speed of the ball milling is 500 rpm, the time of the ball milling is 2 h, the diameter of the ball milling zirconium beads is 10 mm, and the ball-to-material ratio of the ball milling is 30:1; the preset temperature of the roll pressing is 80°C; the roll pressing is performed until the mass mixture has a surface capacity of 2 mAh·cm -2 .
[0062] Positive electrode
[0063] In the positive electrode sheet provided in the second aspect of the present invention, the positive electrode sheet comprises the composite positive electrode material as described above.
[0064] In the present invention, in the positive electrode sheet, the composite positive electrode material is located on at least one side of the positive electrode current collector.
[0065] In the present invention, the positive electrode current collector is used as a substrate for supporting the positive electrode active material layer, and is generally a metal foil with a thickness of 3μm-500μm. There is no particular restriction on the material, as long as it has high conductivity and does not produce chemical reactions in the secondary battery system. For example, it can be a foil formed after surface treatment of nickel, titanium, aluminum, nickel, silver, stainless steel, carbon, etc. The positive electrode current collector is generally a smooth surface, but fine lines can also be formed on its surface to increase the adhesion between the positive electrode active material and the current collector. In addition to the foil, the positive electrode current collector can also be used in any one or more combinations of various forms such as film, mesh, porous, foam or non-woven fabric. Generally, the positive electrode current collector is aluminum foil.
[0066] In a preferred embodiment, the positive electrode current collector is carbon-coated aluminum foil.
[0067] In a preferred embodiment, the thickness of the positive electrode current collector is 6-20 μm, for example, 12 μm.
[0068] In some optional embodiments, the method for preparing the positive electrode sheet comprises the following steps:
[0069] The composite positive electrode material and the positive electrode current collector are composited in a glove box.
[0070] In some preferred embodiments, the atmosphere of the glove box is argon.
[0071] In some preferred embodiments, the dew point temperature of the glove box is -80°C to -40°C, for example -60°C.
[0072] Solid-state lithium-ion battery
[0073] In the solid-state lithium-ion battery provided in the third aspect of the present invention, the solid-state lithium-ion battery comprises the positive electrode sheet, the solid electrolyte layer and the negative electrode sheet as described above.
[0074] Negative plate
[0075] In the present invention, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector.
[0076] In some embodiments, the negative electrode active material layer includes a negative electrode active material.
[0077] The negative electrode active material may be a conventional negative electrode active material of a lithium ion battery in the art. The negative electrode active material of the lithium ion battery may use a compound that can reversibly insert and remove lithium, and specific examples include but are not limited to: graphite materials and / or silicon materials.
[0078] In some preferred embodiments, the graphite material includes one or both of natural graphite and artificial graphite.
[0079] In some more preferred embodiments, the natural graphite includes one or more of block graphite, flake graphite and earthy graphite.
[0080] In some more preferred embodiments, the artificial graphite includes one or more of single crystal graphite, polycrystalline graphite, pyrolytic graphite and graphite fiber.
[0081] In some preferred embodiments, the silicon material includes, but is not limited to, crystalline silicon, amorphous silicon and organic silicon.
[0082] In some embodiments, the negative electrode active material layer further includes a conductive agent.
[0083] Among them, the type of the conductive agent is not particularly limited, and can be selected from graphite materials such as natural graphite and artificial graphite, carbon black SP, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black and other carbon black materials, carbon fibers, metal fibers and other conductive fibers, metal powders such as carbon fluoride powder, aluminum powder, nickel powder and other metal powders, zinc oxide, potassium titanate and other conductive whiskers, and titanium dioxide and other conductive metal oxides or polyphenylene derivatives.
[0084] In some embodiments, the negative electrode active material layer further includes a binder.
[0085] Among them, the type of the binder is not particularly limited, and can be selected from polyvinylidene fluoride, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer and its sulfonate, styrene-butadiene rubber, fluororubber and various copolymers.
[0086] In some embodiments, the negative electrode active material layer further includes a thickener, such as sodium carboxymethyl cellulose.
[0087] In the present invention, the negative electrode current collector may be a conventional negative electrode current collector in the art. The negative electrode current collector is a substrate supporting the negative electrode active material, and is generally a metal foil having a thickness of 3-500 microns. There is no particular restriction on the material, as long as it has high conductivity and does not produce chemical reactions in the power battery system. For example, it can be a foil formed after surface treatment of nickel, titanium, aluminum, nickel, silver, stainless steel, carbon, etc. The negative electrode current collector is generally a smooth surface, but fine lines may also be formed on its surface to increase the adhesion between the positive electrode active material and the current collector. In addition to the foil, the negative electrode current collector may also be used in any one or more combinations of various forms such as film, mesh, porous, foam or non-woven fabric. Generally, the negative electrode current collector is copper foil.
[0088] In the present invention, the preparation method of the negative electrode sheet generally comprises the following steps: the components of the negative electrode active material layer are fully stirred and mixed in a solvent to obtain a negative electrode slurry which is applied on at least one surface of the negative electrode current collector, dried, cold pressed, and cut to obtain the negative electrode sheet.
[0089] In other embodiments, the negative electrode is a metal electrode, which may be indium, lithium, indium, aluminum, or an alloy of at least two of the above metals.
[0090] In a specific embodiment, the negative electrode sheet is a lithium-indium alloy sheet; the diameter of the lithium-indium alloy sheet is, for example, 10 mm.
[0091] Solid electrolyte layer
[0092] In the present invention, the solid electrolyte layer in the solid-state lithium-ion battery includes conventional solid electrolytes in the art.
[0093] In some optional embodiments, the solid electrolyte layer includes a sulfide solid electrolyte, and the solid electrolyte layer is a sulfide solid electrolyte layer.
[0094] In some embodiments, the sulfide solid electrolyte layer includes a sulfide solid electrolyte and a binder.
[0095] In some preferred embodiments, the sulfide solid electrolyte includes Li 10 GeP2S 12 、Li7P3S 11 , one or more of Li6PS5Cl, Li6PS5Br and Li6PS5I.
[0096] In some preferred embodiments, the binder includes one or more of nitrile rubber, styrene butadiene rubber, linear triblock copolymer, polyvinylidene fluoride and polytetrafluoroethylene.
[0097] In some preferred embodiments, the mass ratio of the sulfide solid electrolyte to the binder is (90-100): (0-10).
[0098] In some specific embodiments, in the sulfide solid electrolyte layer, the sulfide solid electrolyte is Li6PS5Cl, the binder is PTFE, and the mass ratio of Li6PS5Cl to PTFE is, for example, 99:1.
[0099] In some embodiments, the method for preparing the sulfide solid electrolyte layer comprises the following steps:
[0100] S1. Mixing the components of the sulfide solid electrolyte layer in a glove box to form a mixture;
[0101] S2, ball milling the mixture to obtain a mass-like mixture;
[0102] S3, rolling the mass mixture to obtain.
[0103] In some preferred embodiments, in step S1, the atmosphere of the glove box is argon.
[0104] In some preferred embodiments, in step S1, the dew point temperature of the glove box is -80°C to -40°C, for example, -60°C.
[0105] In some preferred embodiments, in step S2, the rotation speed of the ball milling treatment is 100-1000 rpm, for example, 500 rpm; the time of the ball milling treatment is 0.5-3 h, for example, 2 h; the diameter of the zirconium beads for the ball milling treatment is 5 mm-20 mm, for example, 10 mm; the ball-to-material ratio of the ball milling treatment is (20-50):1, for example, 30:1.
[0106] In some preferred embodiments, in step S3, the preset temperature of the rolling is 60°C-120°C, for example, 100°C.
[0107] In some preferred embodiments, in step S3, the rolling is performed until the thickness of the mass mixture is 10 μm-200 μm, for example, 50 μm.
[0108] In a specific embodiment, the preparation method of the sulfide solid electrolyte layer comprises the following steps: mixing Li6PS5Cl and PTFE in a glove box and then ball-milling to obtain a lumpy mixture, the ball milling speed is 500 rpm, the ball milling time is 2 h, the diameter of the ball milling zirconium beads is 10 mm, and the ball-to-material ratio is 30:1; rolling the lumpy mixture to 50 μm at 100°C to obtain.
[0109] In some optional embodiments, the method for preparing the solid-state lithium-ion battery comprises the following steps:
[0110] In a glove box, the positive electrode sheet, the sulfide solid electrolyte layer and the negative electrode sheet are sequentially placed into a mold for assembly; after assembly, pressurize and tighten the nut at the top of the column to a constant pressure to obtain the product.
[0111] In some preferred embodiments, the atmosphere of the glove box is argon.
[0112] In some preferred embodiments, the dew point temperature of the glove box is -80°C to -40°C, for example -60°C.
[0113] In some preferred embodiments, the pressurization is pressurization to 1 MPa-200 MPa.
[0114] In some preferred embodiments, the diameters of the positive electrode sheet, the sulfide solid electrolyte layer and the negative electrode sheet are, for example, 10 mm.
[0115] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention. The present invention is further illustrated by way of examples below, but the present invention is not limited to the scope of the embodiments described. The experimental methods in the following examples that do not specify specific conditions are selected according to conventional methods and conditions, or according to the product specifications. Unless otherwise specified, the reagents and raw materials used in the present invention are commercially available.
[0116] The main reagents used in the following examples and comparative examples are as follows:
[0117] Super P was purchased from Tianjin Youmeng Chemical Technology Co., Ltd., model number is Super P;
[0118] VGCF was purchased from Showa Denko K.K., model number VGCF-H;
[0119] PTFE was purchased from Daikin Fluorochemical (China) Co., Ltd., model M-392;
[0120] LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), ZrO2 coated NCM811, Nb2O5 coated NCM811, LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), ZrO2 coated NCM622, LiNi 0.5 Mn 1.5O4 (LNMO) and ZrO2-coated LNMO were purchased from Xiamen Tungsten Co., Ltd.;
[0121] Li6PS5Cl was purchased from Shandong Xinjieneng Lithium Battery Co., Ltd.
[0122] Example 1
[0123] (1) Preparation of the first positive electrode material particles
[0124] S1. At room temperature, 0.17 g of trimesic acid was completely dissolved in 25 mL of N,N-dimethylformamide to obtain a trimesic acid solution. The dissolution time was 1 h. Then 1.5 g of LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) and trimesic acid solution were mixed and stirred for 12 h to form a mixed solution 1;
[0125] S2. At room temperature, completely dissolve 1.05 g zirconium chloride in 45 mL acetic acid for 1 h to obtain a mixed solution 2.
[0126] S3. Stir the mixed solution 1 and the mixed solution 2 at 120°C for 72 h to allow trimesic acid to react with metal ions to generate MOF (MOF-808); then filter the mixed solution, wash the filtrate with acetone, and then vacuum dry at 100°C for 6 h to obtain MOF-808-coated NCM811.
[0127] Among them, the Dv50 of the first positive electrode material core NCM811 is 10.4 μm, and the thickness of the first coating layer is 30 nm.
[0128] (2) Preparation of composite cathode materials
[0129] The following preparation processes of the composite cathode materials were all carried out in a glove box (argon atmosphere, dew point temperature of -60°C).
[0130] S1. Mix the first positive electrode material particles, the second positive electrode material particles (ZrO2-coated NCM811), Li6PS5Cl, Super P, VGCF and PTFE (100 parts by mass in total) in a mass ratio of 55:20:20:2:2:1 to form a mixture;
[0131] S2, ball milling the mixture to obtain a mass-shaped mixture; wherein the rotation speed of the ball milling is 500 rpm, the ball milling time is 2 h, the diameter of the ball milling zirconium bead is 10 mm, and the ball-to-material ratio is 30:1;
[0132] S3. Repeatedly roll the dough mixture at 80°C until the surface capacity reaches 2 mAh·cm-2 , and obtain a composite positive electrode material.
[0133] Among them, the Dv50 of the second positive electrode material core NCM811 in the second positive electrode material particle is 3.3 μm, and the thickness of the second coating layer ZrO2 is 10 nm.
[0134] Among them, the Dv50 of Li6PS5Cl is 1.3 μm, 1 μm<Dv90<1.5 μm, 0.6 μm<Dv10<0.8 μm, and 1.7<Dv90 / Dv10<1.9.
[0135] (3) Preparation of positive electrode
[0136] In a glove box (argon atmosphere, dew point temperature = -60°C), the composite positive electrode material was compounded with 12 μm carbon-coated aluminum foil to obtain a positive electrode sheet, which was then cut into discs with a diameter of 10 mm.
[0137] (4) Preparation of solid-state lithium-ion batteries
[0138] In a glove box (argon atmosphere, dew point temperature = -60°C), the positive electrode sheet, sulfide solid electrolyte layer and negative electrode sheet (lithium indium alloy sheet, disc with a diameter of 10 mm) are placed into the mold in sequence for assembly; after assembly, the pressure is increased to 100 MPa and the nut at the top of the column is tightened to maintain a constant pressure.
[0139] Among them, the preparation method of the sulfide solid electrolyte layer includes the following steps: mixing Li6PS5Cl (Dv50 is 3 μm) with PTFE in a mass ratio of 99:1 and then ball-milling to obtain a lumpy mixture, the rotation speed is 500 rpm, the ball milling time is 2 hours, the diameter of the ball milling zirconium beads is 10 mm, and the ball-to-material ratio is 30:1; repeatedly rolling the lumpy mixture at 100°C to 50 μm to obtain a sulfide solid electrolyte layer, and cutting the sulfide solid electrolyte layer into discs with a diameter of 10 mm.
[0140] Example 2
[0141] The only difference between this embodiment and embodiment 1 is that the type of MOF material in the first positive electrode material particles is MOF-801; when preparing the first positive electrode material particles, zirconium chloride is replaced by zirconium oxychloride octahydrate, and trimesic acid is replaced by fumaric acid; the other conditions remain the same as in embodiment 1.
[0142] Step (1) prepares MOF-801 coated NCM811, wherein the Dv50 of the first positive electrode material core NCM811 is 10.4 μm, and the thickness of the first coating layer is 30 nm.
[0143] Example 3
[0144] The only difference between this embodiment and embodiment 1 is that the second positive electrode material particles are Nb2O5-coated NCM811, and the other conditions are consistent with embodiment 1.
[0145] Among them, the Dv50 of the second positive electrode material core NCM811 is 3.3 μm, and the thickness of the second coating layer Nb2O5 is 10 nm.
[0146] Example 4
[0147] The only difference between this embodiment and embodiment 1 is that the thickness of the first coating layer in the first positive electrode material particles is 10 nm; when preparing the first positive electrode material particles, the amount of N,N-dimethylformamide is replaced by 70 mL, and the amount of acetic acid is replaced by 120 mL; the other conditions are consistent with embodiment 1.
[0148] Example 5
[0149] The only difference between this embodiment and embodiment 1 is that the thickness of the first coating layer in the first positive electrode material particles is 20 nm; when preparing the first positive electrode material particles, the amount of N,N-dimethylformamide is replaced by 50 mL, and the amount of acetic acid is replaced by 90 mL; the other conditions are consistent with embodiment 1.
[0150] Example 6
[0151] The only difference between this embodiment and embodiment 1 is that the thickness of the first coating layer in the first positive electrode material particles is 50 nm; when preparing the first positive electrode material particles, the amount of N,N-dimethylformamide is replaced by 15 mL, and the amount of acetic acid is replaced by 25 mL; the other conditions are consistent with embodiment 1.
[0152] Example 7
[0153] The difference between this embodiment and embodiment 1 is that the thickness of the second coating layer in the second positive electrode material particle is 2 nm, and the other conditions are consistent with embodiment 1. Among them, the Dv50 of the second positive electrode material core NCM811 is 3.3 μm, and the thickness of the second coating layer is 2 nm.
[0154] Example 8
[0155] The only difference between this embodiment and embodiment 1 is that the thickness of the second coating layer in the second positive electrode material particle is 20 nm, and the other conditions are consistent with embodiment 1. Among them, the Dv50 of the second positive electrode material core NCM811 is 3.3 μm, and the thickness of the second coating layer is 20 nm.
[0156] Example 9
[0157] The only difference between this embodiment and Embodiment 1 is that when preparing the composite positive electrode material, the mass ratio of the first positive electrode material particles, the second positive electrode material particles, Li6PS5Cl, Super P, VGCF and PTFE is 45:30:20:2:2:1, and the mass ratio of the first positive electrode material particles to the second positive electrode material particles is 1.5:1, and the other conditions are consistent with Embodiment 1.
[0158] Example 10
[0159] The only difference between this embodiment and Embodiment 1 is that when preparing the composite positive electrode material, the mass ratio of the first positive electrode material particles, the second positive electrode material particles, Li6PS5Cl, Super P, VGCF and PTFE is 67.5:7.5:20:2:2:1, and the mass ratio of the first positive electrode material particles to the second positive electrode material particles is 9:1, and the other conditions are consistent with Embodiment 1.
[0160] Embodiment 11
[0161] The only difference between this embodiment and embodiment 1 is that when preparing the composite positive electrode material, the mass ratio of the first positive electrode material particles, the second positive electrode material particles, Li6PS5Cl, Super P, VGCF and PTFE is 49.8:18.1:27.1:2:2:1, the mass ratio of the corresponding positive electrode material particles and the sulfide solid electrolyte particles is 2.5:1, and the other conditions are consistent with embodiment 1.
[0162] Example 12
[0163] The only difference between this embodiment and Embodiment 1 is that when preparing the composite positive electrode material, the mass ratio of the first positive electrode material particles, the second positive electrode material particles, Li6PS5Cl, Super P, VGCF and PTFE is 34.8:12.7:47.5:2:2:1, the mass ratio of the corresponding positive electrode material particles and the sulfide solid electrolyte particles is 1:1, and the other conditions are consistent with Embodiment 1.
[0164] Example 13
[0165] The only difference between this embodiment and embodiment 1 is that when preparing the composite positive electrode material, the mass ratio of the first positive electrode material particles, the second positive electrode material particles, Li6PS5Cl, Super P, VGCF and PTFE is 62.7:22.8:9.5:2:2:1, the mass ratio of the corresponding positive electrode material particles and the sulfide solid electrolyte particles is 9:1, and the other conditions are consistent with embodiment 1.
[0166] Embodiment 14
[0167] The only difference between this embodiment and embodiment 1 is that the Dv50 of the core of the first positive electrode material is 20 μm, and the other conditions are consistent with those of embodiment 1.
[0168] Step (1) prepares MOF-808 coated NCM811, wherein the Dv50 of the first positive electrode material core NCM811 is 20 μm and the thickness of the first coating layer is 30 nm.
[0169] Embodiment 15
[0170] The only difference between this embodiment and embodiment 1 is that the Dv50 of the core of the first positive electrode material is 15 μm, and the other conditions are consistent with those of embodiment 1.
[0171] Step (1) prepares MOF-808 coated NCM811, wherein the Dv50 of the first positive electrode material core NCM811 is 15 μm and the thickness of the first coating layer is 30 nm.
[0172] Example 16
[0173] The only difference between this embodiment and embodiment 1 is that the Dv50 of the inner core of the second positive electrode material is 2 μm, and the other conditions are consistent with those of embodiment 1.
[0174] The Dv50 of the second positive electrode material core NCM811 is 2 μm, and the thickness of the second coating layer is 10 nm.
[0175] Embodiment 17
[0176] The only difference between this embodiment and embodiment 1 is that the Dv50 of the inner core of the second positive electrode material is 5 μm, and the other conditions are consistent with those of embodiment 1.
[0177] The Dv50 of the second positive electrode material core NCM811 is 5 μm, and the thickness of the second coating layer is 10 nm.
[0178] Embodiment 18
[0179] The only difference between this embodiment and embodiment 1 is that the Dv50 of Li6PS5Cl in the composite positive electrode material is 1.1 μm, and the other conditions are consistent with those in embodiment 1.
[0180] Embodiment 19
[0181] The only difference between this embodiment and embodiment 1 is that the Dv50 of Li6PS5Cl in the composite positive electrode material is 0.6 μm, and the other conditions are consistent with those in embodiment 1.
[0182] Embodiment 20
[0183] The difference between this embodiment and embodiment 1 is only that:
[0184] Using LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622, Dv50 is 9 μm) replaces the first positive electrode material core NCM811 of Example 1, and step (1) prepares MOF-808-coated NCM622, wherein the first positive electrode material core NCM622 and the thickness of the first coating layer are 30 nm;
[0185] The second positive electrode material particles of Example 1 are replaced by NCM622 coated with ZrO2 (the Dv50 of NCM622 is 3.5 μm, and the thickness of the second coating layer ZrO2 is 10 nm);
[0186] The remaining conditions remain the same as those in Example 1.
[0187] Embodiment 21
[0188] The difference between this embodiment and embodiment 1 is only that:
[0189] Using LiNi 0.5 Mn 1.5 O4 (LNMO, Dv50 is 10.4 μm) replaces the first positive electrode material core NCM811 of Example 1 to prepare the first positive electrode material particles; step (1) prepares MOF-808-coated LNMO, wherein the Dv50 of the first positive electrode material core LNMO is 10.4 μm and the thickness of the first coating layer is 30 nm;
[0190] The second positive electrode material particles of Example 1 were replaced by LNMO coated with ZrO2 (Dv50 of LNMO was 3.3 μm, and the thickness of the second coating layer ZrO2 was 10 nm), and the other conditions were the same as those of Example 1.
[0191] Embodiment 22
[0192] The difference between this embodiment and embodiment 1 is that the composite positive electrode material is prepared under a dew point temperature of 0° C., and it should be noted that the dew point temperature during the preparation of the solid-state lithium-ion battery is −60° C. The other conditions are the same as those in embodiment 1.
[0193] Embodiment 23
[0194] The difference between this embodiment and embodiment 1 is that during the preparation process of the solid-state lithium-ion battery, the pressure is increased to 5 MPa after assembly. The other conditions are the same as those in embodiment 1.
[0195] Comparative Example 1
[0196] The difference between this comparative example and Example 1 is that the first positive electrode material particles and the second positive electrode material particles of Example 1 are replaced by ZrO2-coated NCM811 (the Dv50 of NCM811 is 10.7 μm and the thickness of the coating layer is 10 nm). When preparing the composite positive electrode material, the mass ratio of ZrO2-coated NCM811, Li6PS5Cl, Super P, VGCF and PTFE is 75:20:2:2:1, and the other conditions are the same as those of Example 1.
[0197] Comparative Example 2
[0198] The difference between this comparative example and Example 1 is that NCM811 coated with MOF-808 (the Dv50 of NCM811 is 10.4 μm, and the thickness of the MOF-808 coating layer is 30 nm) is used to replace the second positive electrode material particles of Example 1, and the other conditions are consistent with Example 1.
[0199] Comparative Example 3
[0200] The difference between this comparative example and Example 1 is that NCM811 coated with MOF-808 (the Dv50 of NCM811 is 3.3 μm, and the thickness of the coating layer is 30 nm) is used to replace the second positive electrode material particles of Example 1, and the other conditions are consistent with Example 1.
[0201] Comparative Example 4
[0202] The difference between this comparative example and Example 1 is that the first positive electrode material particles of Example 1 are replaced by ZrO2-coated NCM811 (the Dv50 of NCM811 is 10.7 μm, and the thickness of the coating layer is 10 nm), and the other conditions are the same as those of Example 1.
[0203] Comparative Example 5
[0204] The only difference between this comparative example and Example 1 is that the first positive electrode material particles of Example 1 are replaced by NCM811 coated with ZrO2 (the Dv50 of NCM811 is 10.4 μm, and the thickness of the coating layer is 10 nm), and the second positive electrode material particles of Example 1 are replaced by NCM811 coated with MOF-808 (the Dv50 of NCM811 is 3.3 μm, and the thickness of the coating layer is 30 nm), and the other conditions are consistent with Example 1.
[0205] Comparative Example 6
[0206] The only difference between this comparative example and Example 1 is that NCM811 (Dv50 is 10.4 μm) is used to replace the first positive electrode material particles in Example 1, and MOF-808-coated NCM811 (Dv50 of NCM811 is 3.3 μm, and the thickness of the second coating layer is 30 nm) is used to replace the second positive electrode material particles in Example 1, and the other conditions are consistent with Example 1.
[0207] Comparative Example 7
[0208] The difference between this comparative example and Example 1 is that NCM811 (the Dv50 of NCM811 is 3.3 μm) is used to replace the second positive electrode material particles in Example 1, and the other conditions are the same as those in Example 1.
[0209] Comparative Example 8
[0210] The difference between this comparative example and Example 1 is that NCM811 (Dv50 is 10.4 μm) is used to replace the first positive electrode material particles in Example 1, and the other conditions are the same as those in Example 1.
[0211] Comparative Example 9
[0212] The only difference between this comparative example and Example 1 is that the Dv50 of Li6PS5Cl in the composite positive electrode material is 5μm (the particle size is larger than the inner core of the second positive electrode material), 3μm<Dv90<8μm, 1μm<Dv10<3μm, 4<Dv90 / Dv10<5; the Dv50 of Li6PS5Cl in the sulfide solid electrolyte layer is 5μm, and the other conditions are consistent with Example 1.
[0213] Comparative Example 10
[0214] The only difference between this comparative example and Example 1 is that the Dv50 of the core of the second positive electrode material is 14 μm (the particle size is larger than that of the core of the first positive electrode material), and the other conditions are consistent with Example 1.
[0215] Among them, the Dv50 of the second positive electrode material core NCM811 is 14 μm, and the thickness of the second coating layer ZrO2 is 10 nm.
[0216] Comparative Example 11
[0217] The only difference between this comparative example and Example 22 is that NCM811 is used to replace the first positive electrode material particles and the second positive electrode material particles in Example 22, and the other conditions remain the same as Example 22.
[0218] Comparative Example 12
[0219] The only difference between this comparative example and Example 23 is that NCM811 is used to replace the first positive electrode material particles and the second positive electrode material particles in Example 23, and the other conditions are consistent with Example 23.
[0220] Comparative Example 13
[0221] The only difference between this comparative example and Example 23 is that ZrO2-coated NCM811 (the Dv50 of NCM811 is 10.7 μm, and the thickness of the ZrO2 coating layer is 10 nm) is used to replace the first positive electrode material particles in Example 23, and the other conditions remain the same as those in Example 23.
[0222] Comparative Example 14
[0223] The only difference between this comparative example and Example 21 is that LNMO is used to replace the first positive electrode material particles and the second positive electrode material particles in Example 21, and the other conditions remain the same as in Example 21.
[0224] Comparative Example 15
[0225] The difference between this embodiment and embodiment 20 is only that:
[0226] Using LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622, Dv50 is 9 μm) replaces the first positive electrode material particles of Example 20;
[0227] The second positive electrode material particles of Example 20 are replaced with NCM622 (the Dv50 of NCM622 is 3.5 μm);
[0228] The remaining conditions remain the same as in Example 20.
[0229] Effect Example 1
[0230] Number of cycles at room temperature (capacity retention rate is 80%) and first cycle discharge specific capacity
[0231] At 25°C, the solid-state lithium-ion batteries prepared in Examples 1-23 and Comparative Examples 1-15 were subjected to long cycle charge and discharge tests after being constant in capacity, and the number of normal temperature cycles when the first cycle discharge specific capacity and the capacity retention rate were 80% were recorded. Among them, the constant capacity ratio was 0.1°C, and the normal temperature cycle test ratio was 0.3°C.
[0232] When the positive electrode material is NCM811 or NCM622, the operating voltage range is 1.9~3.7 V.
[0233] When the positive electrode material is LNMO, the operating voltage range corresponding to Example 21 and Comparative Example 11 is 1.4~4.25 V.
[0234] The above test results are shown in Table 1.
[0235]
[0236] The composite positive electrode material of the present invention uses a MOF material with flexible characteristics and porous structure to coat a positive electrode material to obtain large particles (first positive electrode material particles), and uses a metal oxide to coat another positive electrode material to obtain small particles (second positive electrode material particles). Among them, small particles are conducive to physical isolation, thereby avoiding side reactions between the positive electrode material and the electrolyte; at the same time, large particles can stabilize the structure of the composite positive electrode material and efficiently utilize high-voltage positive electrode materials with high discharge specific capacity, so that the prepared solid-state lithium-ion battery can significantly improve the cycle performance while ensuring excellent first-cycle discharge specific capacity.
[0237] When NCM811 is used as the positive electrode material, the number of room temperature cycles (capacity retention rate is 80%) of the solid-state lithium-ion battery obtained using the composite positive electrode material in Examples 1-19 can reach more than 200 cycles, and the first cycle discharge specific capacity can reach more than 165 mAh / g.
[0238] Compared with Example 1, when only NCM811 coated with ZrO2 (Comparative Example 1) or only NCM811 coated with MOF-808 (Comparative Example 2) is used as the composite positive electrode material of the positive electrode material particles, the first discharge capacity and the number of cycles at room temperature of the obtained solid-state lithium-ion battery are significantly reduced. When MOF-808 is used to coat two positive electrode materials (Comparative Example 3) or ZrO2 is used to coat two positive electrode materials (Comparative Example 4) to obtain a composite positive electrode material, the first discharge capacity and the number of cycles at room temperature of the obtained solid-state lithium-ion battery are also significantly reduced.
[0239] Compared with Example 1, when only small particles obtained by coating one positive electrode material with MOF and another positive electrode material without coating (Comparative Example 6), only large particles obtained by coating one positive electrode material with MOF and another positive electrode material without coating (Comparative Example 7), or only small particles obtained by coating one positive electrode material with ZrO2 and another positive electrode material without coating (Comparative Example 8) are used as composite positive electrode materials of positive electrode material particles, the first discharge capacity and the number of cycles at room temperature of the obtained solid-state lithium-ion battery are also greatly reduced. Even if MOF-808 and ZrO2 are used to coat the two positive electrode materials respectively, compared with Example 1, the large particles obtained by coating one positive electrode material with ZrO2 and the small particles obtained by coating another positive electrode material with MOF-808 in Comparative Example 5 cannot take into account both the excellent first discharge capacity and the number of cycles at room temperature.
[0240] From the comparison between Comparative Examples 1-8 and Example 1, it can be seen that only by using a composite positive electrode material obtained by coating a large particle of a positive electrode material with a MOF material and a small particle of another positive electrode material with a metal oxide to obtain a composite positive electrode material, can the obtained solid-state lithium-ion battery have both excellent first-cycle discharge capacity and number of cycles at room temperature. Among them, the small particles fill the pores of the large particles, which can reduce the porosity of the composite positive electrode material, reduce the amount of solid electrolyte used in the composite positive electrode material, and improve the utilization rate of the positive electrode material particles; more importantly, the composite positive electrode material has good consistency in dimensions such as expansion degree and breakage rate, which can ensure the structural stability of the obtained positive electrode sheet, and improve the cycle performance of the solid-state lithium-ion battery while ensuring the discharge capacity.
[0241] By comparing Example 1 and Comparative Example 9, it can be seen that when the Dv50 of the sulfide solid electrolyte particles in the composite positive electrode material is greater than the Dv50 of the second positive electrode material core, the first-cycle discharge capacity and the number of cycles at room temperature of the obtained solid-state lithium-ion battery are greatly reduced. This may be because when the Dv50 of the sulfide solid electrolyte particles is too large, the utilization rate of the positive electrode material particles decreases, the porosity of the composite positive electrode material increases, and the ion transmission path decreases, thereby deteriorating the battery performance. Similarly, when the Dv50 of the second positive electrode material core is greater than the Dv50 of the first positive electrode material core (Comparative Example 10), it is also impossible to take into account both the excellent first-cycle discharge capacity and the number of cycles at room temperature.
[0242] It can be seen from Comparative Example 11 and Example 22 that even if the solid composite cathode material is assembled in an environment with a dew point temperature of 0°C, the solid lithium-ion battery still has good capacity and cycle performance; it can be seen from Comparative Examples 12-13 and Example 23 that even when the pressure applied to the outside of the battery is small (5 MPa), the solid lithium-ion battery still has good discharge specific capacity and cycle performance. It can be seen from the above that in the composite cathode material of the present invention, the first coating layer obtained from the MOF material with porous and flexible characteristics plays a key role in the high performance of the battery, which ensures the practicality of the composite cathode material.
[0243] The composite positive electrode material of the present invention is suitable for various positive electrode active materials of lithium ion batteries. Taking NCM622 as the positive electrode active material as an example, it can be seen from Examples 1 and 20 that when the Ni content of the positive electrode active material is reduced, although the discharge specific capacity and the number of cycles at room temperature of the obtained solid-state lithium ion battery are reduced, compared with the case of the uncoated positive electrode material in Comparative Example 15, its discharge specific capacity and the number of cycles at room temperature are still very excellent. Taking LNMO as the positive electrode active material as an example, it can be seen from Comparative Example 14 and Example 21 that the solid-state lithium ion battery prepared using the composite positive electrode material of the present invention also has relatively excellent discharge specific capacity and cycle performance.
[0244] For the composite positive electrode material of the present invention, the type of MOF material in the first coating layer and the type of metal oxide in the second coating layer have little effect on the first cycle discharge capacity and cycle performance of the obtained solid-state lithium-ion battery. Taking Example 2 as an example, when the first coating layer uses different types of MOF materials such as MOF-801, the obtained solid-state lithium-ion battery can also significantly improve the cycle performance while ensuring excellent first cycle discharge capacity. Similarly, when the second coating layer uses different types of metal oxides such as Nb2O5 (Example 3), the obtained solid-state lithium-ion battery also has excellent first cycle discharge capacity and cycle performance.
[0245] There is a preferred range for the thickness of the first coating layer and the thickness of the second coating layer in the composite positive electrode material of the present invention. Within this range, the obtained solid-state lithium-ion batteries have relatively excellent first-cycle discharge capacity and cycle performance. In Examples 4-6, as the thickness of the first coating layer increases, the first-cycle discharge capacity decreases, while the number of cycles at room temperature gradually increases. In Examples 7-8, compared with Example 1, when the thickness of the first coating layer becomes appropriately smaller or larger, the first-cycle discharge capacity decreases, while the number of cycles at room temperature decreases or increases accordingly.
[0246] The mass ratio of the first positive electrode material particles and the second positive electrode material particles, and the mass ratio of the positive electrode material particles and the solid electrolyte particles in the composite positive electrode material of the present invention have a preferred range, and the first discharge capacity and cycle performance of the corresponding solid-state lithium ion battery are relatively excellent. Compared with Example 1, when the mass ratio of the first positive electrode material particles and the second positive electrode material particles in Example 9 is appropriately reduced, the first discharge capacity is reduced, and the number of cycles at room temperature is increased accordingly; when the mass ratio of the first positive electrode material particles and the second positive electrode material particles in Example 10 is appropriately increased, the first discharge capacity and the number of cycles at room temperature are reduced, but also within the excellent range; when the mass ratio of the positive electrode material particles and the solid electrolyte particles in Examples 11-12 is appropriately reduced, the first discharge capacity and the number of cycles at room temperature are increased; in Example 13, when the mass ratio of the positive electrode material particles and the solid electrolyte particles is appropriately increased, the first discharge capacity and the number of cycles at room temperature are reduced, but also relatively excellent.
[0247] In addition, there are also preferred ranges for the Dv50 of the core of the first positive electrode material, the Dv50 of the core of the second positive electrode material, and the Dv50 of Li6PS5Cl, and the resulting solid-state lithium-ion battery can have both excellent first-cycle discharge capacity and cycle performance. In Examples 14-17, when the Dv50 of the core of the first positive electrode material is appropriately increased (Examples 14-15) or the Dv50 of the core of the second positive electrode material is appropriately increased (Example 16) or decreased (Example 17), the first-cycle discharge capacity and number of cycles at room temperature of the resulting solid-state lithium-ion battery are reduced; for Examples 18-19, when the Dv50 of Li6PS5Cl is appropriately increased or decreased, the first-cycle discharge capacity and number of cycles at room temperature of the resulting solid-state lithium-ion battery are increased.
[0248] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A composite positive electrode material, It is characterized in that It includes positive electrode material particles and solid electrolyte particles; The positive electrode material particles include a first positive electrode material particle and a second positive electrode material particle; the first positive electrode material particle includes a first positive electrode material core and a first coating layer; the second positive electrode material particle includes a second positive electrode material core and a second coating layer; Wherein, the first coating layer comprises MOF material; the second coating layer comprises metal oxide; The particle size of the core of the first positive electrode material is larger than that of the core of the second positive electrode material; and the particle size of the core of the second positive electrode material is larger than that of the solid electrolyte particles.
2. The composite cathode material according to claim 1, It is characterized in that The thickness of the first coating layer is 10nm-50nm; the thickness of the second coating layer is 2nm-20nm.
3. The composite positive electrode material according to claim 1, It is characterized in that The Dv50 of the inner core of the first positive electrode material is 8 μm-20 μm; the Dv50 of the inner core of the second positive electrode material is 2 μm-5 μm; and the Dv50 of the solid electrolyte particles is 0.6 μm-1.5 μm.
4. The composite cathode material according to claim 1, It is characterized in that The particle size of the solid electrolyte particles satisfies: 1.7<Dv90 / Dv10<1.9; 1μm<Dv90<1.5μm; 0.6μm<Dv10<0.8μm.
5. The composite cathode material according to claim 1, It is characterized in that The content of the first positive electrode material particles is 30%-90%, the content of the second positive electrode material particles is 5%-40%, and the content of the solid electrolyte particles is 5%-50%, where the percentages are the mass percentages of each component in the composite positive electrode material.
6. The composite cathode material according to claim 1, It is characterized in that The MOF material includes one or both of a zirconium-based MOF material and a chromium-based MOF material; The metal oxide includes one or more of zinc oxide, tin oxide, titanium oxide, copper oxide, tungsten oxide, zirconium oxide, aluminum oxide and niobium oxide.
7. The composite cathode material according to claim 1, It is characterized in that The composite positive electrode material satisfies one or more of the following conditions ad: a. The first positive electrode material core and the second positive electrode material core each independently include one or more of lithium nickel cobalt manganese oxide, lithium nickel manganese oxide, lithium iron phosphate, lithium manganese iron phosphate and lithium cobalt oxide; b. The solid electrolyte particles are sulfide solid electrolyte particles, and the sulfide solid electrolyte particles include Li 10 G 2 S 12 , Li 7 P 3 S 11 , Li 6 PS 5 Cl, Li 6 PS 5 Br and Li 6 PS 5 One or more of I; c. The composite positive electrode material further includes a conductive agent, which includes one or more of graphite, graphene, carbon black, carbon fiber and carbon nanotubes; the content of the conductive agent is 1%-5%, where the percentage is the mass percentage of the composite positive electrode material; d. The composite positive electrode material also includes a binder, which includes one or more of polytetrafluoroethylene, styrene-butadiene rubber, ethylene-tetrafluoroethylene copolymer and ethylene-chlorotrifluoroethylene copolymer; the content of the binder is 0.1%-2%, and the percentage is the mass percentage of the composite positive electrode material.
8. A positive electrode sheet, It is characterized in that It comprises the composite positive electrode material as claimed in any one of claims 1 to 7.
9. A solid-state lithium-ion battery, It is characterized in that It comprises the positive electrode sheet, a solid electrolyte layer and a negative electrode sheet as claimed in claim 8.
10. The solid-state lithium-ion battery according to claim 9, It is characterized in that The solid electrolyte layer includes a sulfide solid electrolyte.