A sand control method for fracturing tail chasing
By using high-purity quartz sand and phenolic resin in fracturing tail chasing, combining coupling agents and accelerators, the problem of resin-coated sand cementation at different temperatures is solved, and uniform cementation and high temperature oil wells are achieved in ultra-low temperature and high temperature oil wells Strength, suitable for sand prevention construction of various well types.
Patent Information
- Application Number
- CN202411102696.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The existing fracturing tail-track resin sand-proofing process is the problem of wasting amounts or insufficient curing strength in ultra-low and high-temperature oil wells due to different temperatures, which leads to waste of dosage or insufficient curing strength.
High-purity quartz sand is mixed with phenolic resin solution, coupling agent and accelerator are added, resin-coated sand is prepared by vibrating air-cooled bed drying, and the concentration of curing agent is adjusted by temperature changes to ensure effective cementation at different temperatures.
It realizes uniform cementation of resin-coated sand at different temperatures, improves curing strength and adaptability, and is suitable for sand-proof construction at different depths and well types, with excellent chemical stability and corrosion resistance.
Smart Images

Figure SMS_3 
Figure SMS_4 
Figure SMS_5
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sand control for oil, water and gas wells, and in particular to a sand control method for fracturing tail chasing. Background Art
[0002] Problems such as proppant spitting and formation sand production after fracturing of oil and gas wells have always restricted the normal performance of oil well production capacity. In mild cases, it can affect the normal production of oil and gas wells, and in severe cases, it can lead to the scrapping of oil and gas wells. In particular, chemical sand control for ultra-low temperature oil and gas wells is even more difficult. With the continuous improvement of sand control technology, the fracturing tail chase resin coated sand sand control technology has been increasingly recognized and applied. Only by taking proactive sand control in advance can the oil well production capacity be truly improved, the later operations can be reduced, and the maintenance cost can be reduced. At present, the use of fracturing tail chase sand coating for sand control in various oil fields across the country has become the main sand control technology to solve the problems of proppant spitting and formation sand production after fracturing of oil and gas wells.
[0003] However, in the existing fracturing tail chase resin coated sand sand control process, the bonding and curing of the coated sand has high requirements on the temperature inside the oil well, that is, the coated sand is easier to bond and cure in high-temperature oil wells, while the bonding and curing time is longer in low-temperature oil wells. In ultra-low temperature oil wells (about 20°C), it is even difficult to bond and cure. In high-temperature oil wells, since the coated sand is easier to bond and cure, this puts forward requirements on the amount of auxiliary agent used in the coated sand. A large amount is likely to cause waste and further increase the cracks in the oil well; while a small amount is likely to lead to the problem of low curing strength of the coated sand.
[0004] Therefore, how to balance the amount of coated sand and its auxiliary agent so that the coated sand can be easily cemented and solidified in both ultra-low temperature oil wells and high temperature oil wells is a difficult problem currently faced in engineering. Summary of the invention
[0005] In view of the above defects, the purpose of the present invention is to provide a fracturing tail chasing sand prevention method, which aims to solve the problem in the prior art that it is difficult to balance the amount of coated sand and its auxiliary agents due to the difference in ambient temperature between ultra-low temperature oil wells and high temperature oil wells.
[0006] In order to solve the above technical problems, the technical solution of the present invention is:
[0007] A fracturing tail-chasing sand control method comprises the following steps:
[0008] Step 1, preparing resin-coated sand;
[0009] The high-purity quartz sand and the phenolic resin solution are sent to a sand mixer for mixing, a coupling agent is added during the mixing process, and a preliminary mixture is obtained after the mixing is completed; the preliminary mixture is sent to a disperser through a conveyor belt for dispersion, and the dispersed preliminary mixture is sent to a vibrating air-cooled bed for drying to obtain resin-coated sand;
[0010] Step 2, preparing a curing agent;
[0011] The accelerator, pH adjuster and polyol are sent to a mixing kettle for stirring and mixing to obtain a curing agent;
[0012] Step 3, crack filling;
[0013] First, high-purity quartz sand is mixed with sand-carrying fluid and then pumped to the cracks of the oil well by a fracturing pump truck, and the high-purity quartz sand is mixed with the original formation to form a mixed sand zone; secondly, the resin-coated sand in step 1 is pumped to the cracks of the oil well by a fracturing pump truck, and then the curing agent in step 2 is sent to the cracks of the oil well by a fracturing pump truck, and the curing agent moves toward the mixed sand zone through the gaps between the resin-coated sands. In this process, the curing agent catalyzes the bonding of the resin-coated sand to form a support zone; finally, the curing agent catalyzes the bonding of the resin-coated sand in the perforated blasthole to form a leakage zone;
[0014] In step 3, the curing agent is mixed with water and then delivered to the crack of the oil well by a fracturing pump truck; the curing agent is mixed with water to obtain a mixed solution, and the concentration of the curing agent in the mixed solution changes with temperature. The calculation formula of the curing agent concentration is:
[0015] ,
[0016] b is the concentration of curing agent, a is the temperature at the oil well fracture (℃), a≥55℃.
[0017] Wherein, in step 1, the sand mixer needs to add phenolic resin powder when mixing high-purity quartz sand and phenolic resin solution, and the weight ratio of phenolic resin solution to phenolic resin powder is 3.6-4.3:0.7-1.4.
[0018] Among them, in the resin-coated sand, the resin coating rate of the quartz sand surface is ≥97%.
[0019] The particle size of the resin-coated sand is 0.3-1.4 mm, the particle dispersion rate of the resin-coated sand is ≥ 98%, and the density of the resin-coated sand is 1.3-1.6 t / m 3 .
[0020] Wherein, the usage ratio of the resin-coated sand to the curing agent is 1-1.2:0.8-1, calculated by usage volume.
[0021] Wherein, at 20°C, the acidity of the curing agent is 0.3-0.6 mol / L, and the density of the curing agent is 0.9 t / m 3 -1.1t / m 3 .
[0022] In step 3, the resin-coated sand is mixed with the sand-carrying fluid and then pumped to the oil well fracture by a fracturing pump truck. The sand ratio of the resin-coated sand in the mixture of the resin-coated sand and the sand-carrying fluid is 30%-70%, and the filling speed of the mixture of the resin-coated sand and the sand-carrying fluid is 2.8-4.2m / s. 3 / min, the conveying pressure of the resin-coated sand is ≤60MPa.
[0023] Among them, the coupling agent is composed of one or more of monoalkoxy titanate, isopropyl tri(dioctyl pyrophosphate acyloxy) titanate, isopropyl dioleyl acyloxy (dioctyl phosphate acyloxy) titanate, γ-aminopropyl triethoxy silane, and γ-aminopropyl methyl diethoxy silane; the accelerator is one or more of formaldehyde, zinc chloride, copper sulfate, and organic acid; the pH adjuster is composed of one or more of citric acid, carbonic acid, silicic acid, and acetic acid; the polyol is composed of one or more of pentaerythritol, glycerol, methyl propylene glycol, ethylene glycol, dipropylene glycol, and neopentyl glycol.
[0024] After adopting the above technical solution, the beneficial effects of the present invention are:
[0025] First, high-quality quartz sand is used as raw material, which can adapt to the fracturing and sand control construction needs of strata at different depths; second, the resin-coated sand has high bonding strength after curing and is not easy to break; third, the construction process is not affected by the number of layers, thickness, and span of the construction well; fourth, the bonding and curing environment has strong adaptability and can adapt to the sand control needs at different temperatures, solving the problem of difficult bonding and curing at low temperatures; fifth, it has a wide range of applications and can be used for vertical, inclined, horizontal wells and window side drilling; sixth, the resin-coated sand after solidification has excellent chemical stability, corrosion resistance, and high structural strength. DETAILED DESCRIPTION
[0026] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.
[0027] Example:
[0028] A fracturing tail-chasing sand control method comprises the following steps:
[0029] Step 1, preparing resin-coated sand;
[0030] High-purity quartz sand and phenolic resin solution are sent to a sand mixer for mixing, a coupling agent is added during the mixing process, and a preliminary mixture is obtained after the mixing is completed; the preliminary mixture is sent to a disperser through a conveyor belt for dispersion, and the dispersed preliminary mixture is sent to a vibrating air-cooled bed for drying to obtain resin-coated sand. Phenolic resin has excellent heat resistance and chemical resistance, can maintain stability under high temperature and chemical corrosion environment, and has good mechanical strength and rigidity. The phenolic resin solution is applied to the surface of the quartz sand through a sand mixer. When the phenolic resin dries on the surface of the quartz sand, the phenolic resin will form a protective film on the surface of the quartz sand, which enhances the corrosion resistance, wear resistance and structural strength of the quartz sand. Although phenolic resin has a certain bonding ability, its bonding ability decreases after drying. For this reason, this scheme introduces a coupling agent.
[0031] In this scheme, the concentration of phenolic resin in the phenolic resin solution is not less than 70%.
[0032] Coupling agents can form chemical bonds or physical adsorption at the interface of two or more different materials (such as organic and inorganic substances), thereby significantly improving the bonding strength between them. This enhanced bonding strength helps to reduce the separation or peeling phenomenon between materials and improve the mechanical properties of the overall material. In addition, coupling agents can reduce the degradation rate of materials under environmental conditions (such as moisture, high temperature or chemical media). By forming a protective coating or interface structure on the surface of the material, coupling agents help to enhance the weather resistance and chemical resistance of the material. Through the dual effects of coupling agents and phenolic resins, the mechanical properties of quartz sand are further improved and its supporting capacity is increased.
[0033] Since coupling agent and phenolic resin easily make high-purity quartz sand stick together to form agglomerates, the agglomerate quartz sand is difficult to be transported to the cracks of oil wells. Therefore, the preliminary mixed materials need to be sent to a disperser to be broken into granular materials, and then the granular materials are sent to a vibrating air-cooled drying bed to remove the moisture contained in the granular materials during vibration to prevent the subsequent granular materials from sticking together again.
[0034] Step 2, preparing a curing agent;
[0035] The accelerator, pH adjuster and polyol are sent to a mixing kettle for stirring and mixing to obtain a curing agent. The function of the curing agent is to activate the coupling agent and the phenolic resin. Under the catalysis of the curing agent, coupled with the temperature and pressure at the cracks of the oil well, the phenolic resin on the surface of the resin-coated sand undergoes a cross-linking reaction to form a macromolecular three-dimensional network structure, which enables the resin-coated sand to be tightly fixed together. Since there are certain gaps between the gravel and the gravel, the consolidated resin-coated sand has a certain percolation ability while having extremely high strength, which allows the oil in the oil well to flow out through the gaps, while the gravel impurities mixed in the oil will be blocked and filtered.
[0036] After the resin-coated sand and the curing agent are prepared, we need to fill them into the cracks of the oil well to support the cracks. To this end, step 3 is also included.
[0037] Step 3, crack filling;
[0038] First, high-purity quartz sand is mixed with sand-carrying fluid and then pumped to the cracks of the oil well by a fracturing pump truck, and the high-purity quartz sand is mixed with the original formation to form a mixed sand zone; secondly, the resin-coated sand in step 1 is pumped to the cracks of the oil well by a fracturing pump truck, and then the curing agent in step 2 is sent to the cracks of the oil well by the fracturing pump truck, and the curing agent moves toward the mixed sand zone through the gaps between the resin-coated sands. In this process, the curing agent catalyzes the bonding of the resin-coated sand to form a support zone; finally, the curing agent catalyzes the bonding of the resin-coated sand in the perforating blasthole to form a leakage zone. The mixed sand belt is formed by mixing quartz sand and formation, and its function is to initially prop up the oil well cracks; the support belt is formed by the combination of resin-coated sand and curing agent, and its function is to support the cracks and prevent the problem of sand backflow in the mixed sand belt; the leakage belt is also formed by the combination of resin-coated sand and curing agent, and there is a gap between the leakage belt and the perforation hole, and its purpose is to increase the seepage area of crude oil, reduce oil flow resistance, and reduce production pressure difference.
[0039] In step 3, when transporting high-purity quartz sand, liquid needs to be placed in advance. The purpose is to squeeze the formation sand at the crack mouth and blasthole into the crack to leave space for subsequent sand injection.
[0040] In this scheme, the resin-coated sand is pumped into the cracks first, and the curing agent is pumped into the cracks after the resin-coated sand is pumped. The purpose of this operation is to prevent the resin-coated sand from cementing and solidifying before entering the cracks when the two are pumped together, making it difficult for the resin-coated sand to enter the cracks through perforations.
[0041] In step 1, the sand mixer needs to add phenolic resin powder when mixing high-purity quartz sand and phenolic resin solution, and the weight ratio of phenolic resin solution to phenolic resin powder is 3.6-4.3:0.7-1.4. The purpose of adding phenolic resin powder is to accelerate the drying speed of the resin-coated sand after coating and reduce the probability of sand and gravel sticking together.
[0042] In order to ensure the strength of the resin coated sand after bonding, the resin coating rate of the quartz sand surface in the resin coated sand should be ≥97%.
[0043] In order to facilitate the pumping of resin-coated sand and avoid the resin-coated sand clogging the perforation, the particle size of the resin-coated sand is 0.3mm-1.4mm, wherein the particle dispersion rate of the resin-coated sand is ≥98%, the purpose of which is to avoid the resin-coated sand sticking together. Preferably, the density of the resin-coated sand is 1.3-1.6t / m 3 .
[0044] At 20°C, the acidity of the curing agent is 0.3-0.6 mol / L, and the density of the curing agent is 0.9 t / m 3 -1.1t / m 3 . Since the formation in the oil well cracks is weakly alkaline, in order to prevent the weak alkaline environment from causing the life of the support belt after bonding to decrease, we need to neutralize the alkaline environment in the cracks. For this reason, the curing agent introduces a pH regulator to adjust the pH value of the curing agent, making the curing agent weakly acidic. During the bonding process of the catalytic resin-coated sand, since the curing agent is a liquid, it will spread through the gaps between the sand and gravel, and eventually contact the formation, thereby causing the alkaline environment to undergo a neutralization reaction, so that the formation in the cracks is no longer weakly alkaline.
[0045] In order to ensure the strength of the support belt, we need to ensure that the resin-coated sand at the support belt can be fully bonded. To this end, the ratio of the resin-coated sand to the curing agent is 1-1.2:0.8-1 based on the usage volume.
[0046] The purpose of the curing agent in this scheme is to ensure that the resin-coated sand can be bonded normally in a low temperature environment (about 20°C), but the curing agent in this scheme can also be used normally in a high temperature environment. However, after many tests, we found that when the temperature is higher than 55°C, the curing agent in this scheme is more active, which makes it easier for the resin-coated sand to bond together. After many experiments, we found that as the temperature rises, we can gradually reduce the concentration of the curing agent. This operation will not lead to a worse bonding effect, but will reduce costs. To this end, in step 3, the curing agent is mixed with water and sent to the cracks of the oil well by a fracturing pump truck; the curing agent is mixed with water to obtain a mixed solution, and the concentration of the curing agent in the mixed solution changes with temperature. The calculation formula for the curing agent concentration is:
[0047] ,
[0048] b is the concentration of curing agent, a is the temperature at the oil well fracture (℃), a≥55℃.
[0049] In this scheme, 55℃ is the starting temperature. It can be seen from the above formula that when the temperature exceeds 55℃, the curing agent concentration should decrease by 20% for every 10℃ increase. When the oil well fracture concentration is lower than 55℃, in order to ensure the consolidation efficiency, the amount of water in the mixed solution of curing agent and water is 0, that is, the concentration of curing agent is 100%.
[0050] In step 3, the resin-coated sand is mixed with the sand-carrying liquid and then pumped to the oil well fracture by a fracturing pump truck. The mixture of the resin-coated sand and the sand-carrying liquid is in a slurry state, which is convenient for the pump truck to discharge the material. The sand ratio of the resin-coated sand in the mixture of the resin-coated sand and the sand-carrying liquid is 30%-50%, and the filling speed of the mixture of the resin-coated sand and the sand-carrying liquid is 2.8-4.2m 3 / min, the conveying pressure of the resin-coated sand is ≤60MPa.
[0051] In order to ensure that the resin-coated sand can be bonded quickly, we need to deliver the curing agent into the crack at a suitable speed. For this purpose, the delivery speed of the curing agent is 0.4-0.6m 3 / min.
[0052] In order to ensure that the resin-coated sand is fully dried and prevent the problem of sand and gravel sticking, the wind speed of the vibrating air-cooling bed is 5000-6000m 3 / h, the working wind pressure is 1.6-2.6KPa.
[0053] A fracturing tail-chasing sand prevention material comprises resin-coated sand and a curing agent, wherein the resin-coated sand comprises phenolic resin, quartz sand and a coupling agent, and the weight ratio of the quartz sand, the phenolic resin and the coupling agent is 8.8-9.2: 0.6-0.8: 0.22-0.28; the curing agent comprises an accelerator, a pH regulator and a polyol, and the weight ratio of the accelerator, the pH regulator and the polyol is 9-9.2: 0.4-0.5: 0.4-0.5.
[0054] The coupling agent is composed of one or more of monoalkoxy titanate, isopropyl tri(dioctyl pyrophosphate acyloxy) titanate, isopropyl dioleyl acyloxy (dioctyl phosphate acyloxy) titanate, γ-aminopropyl triethoxy silane, and γ-aminopropyl methyl diethoxy silane.
[0055] The accelerator is one or more of formaldehyde, zinc chloride, copper sulfate and organic acid.
[0056] The pH regulator is composed of one or more of citric acid, carbonic acid, silicic acid and acetic acid.
[0057] The polyol is composed of one or more of pentaerythritol, glycerol, methyl propylene glycol, ethylene glycol, dipropylene glycol, and neopentyl glycol.
[0058] Embodiment 1:
[0059] In this embodiment, resin-coated sand and a curing agent are produced according to the above scheme and filled into fractures of an oil well.
[0060] The sand ratio of the resin-coated sand in the mixture of the resin-coated sand and the sand-carrying liquid is 50%, and the filling speed of the mixture of the resin-coated sand and the sand-carrying liquid is 2.8 m / s. 3 / min, the conveying pressure of the resin-coated sand is 30MPa. The conveying speed of the curing agent is 0.4m 3 / min. The resin coating rate of the quartz sand surface is 97%, the particle size of the resin coated sand is 0.3mm, the particle dispersion rate of the resin coated sand is 98%, and the density of the resin coated sand is 1.3t / m 3 At 20°C, the acidity of the curing agent is 0.3 mol / L, and the density of the curing agent is 0.9 t / m 3 .
[0061] Calculated by usage volume, the ratio of the resin-coated sand to the curing agent is 1:0.8.
[0062] By weight, the ratio of the quartz sand, phenolic resin and coupling agent is 8.8:0.8:0.28; the ratio of the accelerator, pH regulator and polyol is 9:0.5:0.5.
[0063] The coupling agent is monoalkoxy titanate.
[0064] The accelerator is formaldehyde.
[0065] The pH adjuster is citric acid.
[0066] The polyol is glycerol.
[0067] Embodiment 2:
[0068] The difference between this embodiment and embodiment 1 is that:
[0069] The sand ratio of the resin-coated sand in the mixture of the resin-coated sand and the sand-carrying liquid is 45%, and the filling speed of the mixture of the resin-coated sand and the sand-carrying liquid is 3m 3 / min, the conveying pressure of the resin-coated sand is 35MPa. The conveying speed of the curing agent is 0.45m 3 / min. The resin coating rate of the quartz sand surface is 97.5%, the particle size of the resin coated sand is 0.5mm, the particle dispersion rate of the resin coated sand is 98.5%, and the density of the resin coated sand is 1.4t / m 3 At 20°C, the acidity of the curing agent is 0.5 mol / L, and the density of the curing agent is 1 t / m 3 .
[0070] Calculated by usage volume, the usage ratio of the resin-coated sand to the curing agent is 1.1:0.9.
[0071] Embodiment 3:
[0072] The difference between this embodiment and embodiment 1 is that:
[0073] The sand ratio of the resin-coated sand in the mixture of the resin-coated sand and the sand-carrying liquid is 40%, and the filling speed of the mixture of the resin-coated sand and the sand-carrying liquid is 3.5m 3 / min, the conveying pressure of the resin-coated sand is 40MPa. The conveying speed of the curing agent is 0.5m 3 / min. The resin coating rate of the quartz sand surface is 97.8%, the particle size of the resin coated sand is 0.6mm, the particle dispersion rate of the resin coated sand is 98.7%, and the density of the resin coated sand is 1.5t / m 3 At 20°C, the acidity of the curing agent is 0.55 mol / L, and the density of the curing agent is 1.05 t / m 3 .
[0074] Calculated by usage volume, the usage ratio of the resin-coated sand to the curing agent is 1.15:0.95.
[0075] Embodiment 4:
[0076] The difference between this embodiment and embodiment 1 is that:
[0077] The sand ratio of the resin-coated sand in the mixture of the resin-coated sand and the sand-carrying liquid is 30%, and the filling speed of the mixture of the resin-coated sand and the sand-carrying liquid is 4.2m 3 / min, the conveying pressure of the resin-coated sand is 60MPa. The conveying speed of the curing agent is 0.6m 3 / min. The resin coating rate of the quartz sand surface is 98%, the particle size of the resin coated sand is 1.4mm, the particle dispersion rate of the resin coated sand is 98.9%, and the density of the resin coated sand is 1.6t / m 3 At 20°C, the acidity of the curing agent is 0.6 mol / L, and the density of the curing agent is 1.1 t / m 3 .
[0078] Calculated by usage volume, the ratio of the resin-coated sand to the curing agent is 1.2:1.
[0079] In Examples 1 to 4, the same resin-coated sand and curing agent were used, and only the parameters in the filling process were different.
[0080] Example 1 to Example 4 correspond to well numbers t2036a to t2036d respectively. Statistics of sand prevention effects of oil wells after construction are as follows:
[0081]
[0082] Comparative Example 1:
[0083] The difference between this comparative example and Example 1 is that the resin coating rate on the surface of the quartz sand is 96%.
[0084] The core strength simulation test was carried out by using the resin-coated sand and curing agent in Example 1 and Comparative Example 1, and the results are as follows:
[0085]
[0086] Comparative Example 2:
[0087] The difference between this comparative example and Example 1 is that the resin coating rate on the surface of the quartz sand is 90%.
[0088] The core strength simulation test was carried out by using the resin-coated sand and curing agent in Example 1 and Comparative Example 1, and the results are as follows:
[0089]
[0090] It can be seen from Comparative Examples 1 and 2 that the resin coating rate on the surface of quartz sand will affect the compressive strength of the resin-coated sand after bonding.
[0091] Comparative Example 3:
[0092] This comparative example is different from Example 1 in that the particle size of the resin-coated sand is 0.25 mm.
[0093] Comparative Example 4:
[0094] This comparative example is different from Example 1 in that the particle size of the resin-coated sand is 1.5 mm.
[0095] Comparative Example 5:
[0096] This comparative example is different from Example 1 in that the particle size of the resin-coated sand is 1.6 mm.
[0097]
[0098] Although the core strength of Comparative Examples 3 and 4 is similar to that of Example 1, we found in actual use that the resin-coated sand in Comparative Example 3 requires the sand mixer and the scatterer to work longer, otherwise the particle size cannot reach 0.25 mm. The resin-coated sand in Comparative Examples 4 and 5 needs to use more resin and coupling agent during manufacturing, otherwise the resin coating rate on the surface of the finished resin-coated sand will be lower. Therefore, the particle size of the resin-coated sand is preferably 0.3-1.4 mm.
[0099] Comparative Example 6:
[0100] The difference between this comparative example and Example 1 is that, based on the usage volume, the usage ratio of the resin-coated sand to the curing agent is 0.9:1.1.
[0101] Comparative Example 7:
[0102] The difference between this comparative example and Example 1 is that, based on the usage volume, the usage ratio of the resin-coated sand to the curing agent is 1.3:0.7.
[0103]
[0104] Although the anti-sand effect in Comparative Example 6 is satisfactory, it can be found through comparison that the amount of curing agent used is too much, resulting in excessive cost. In Comparative Example 7, there is a problem of sanding. After investigation and research, we found that due to the small amount of curing agent input, part of the resin-coated sand did not adhere, resulting in a decrease in overall strength, and the gaps between the gravels were too large, resulting in sand problems.
[0105] Comparative Example 8:
[0106] The difference between this comparative example and Example 1 is that the filling speed of the resin-coated sand is 2.5 m / s. 3 The filling speed of the resin-coated sand in this comparative example was too low, resulting in an excessively long construction time.
[0107] Comparative Example 9:
[0108] The difference between this comparative example and Example 1 is that the filling speed of the resin-coated sand is 5m 3 / min. In this comparative example, the filling speed is much higher than the specified speed, so that the cracks are flushed again, resulting in a decrease in crack strength.
[0109] From the comparison of Example 1-Example 2, and Comparative Examples 8 and 9, it can be seen that when the resin-coated sand is filled, the sand ratio used in the slurry mixed with the sand-carrying liquid refers to the volume proportion of the resin-coated sand in the slurry. The larger the sand ratio, the greater the slurry concentration, and the more difficult it is to discharge the material, so a pump truck is required to pump at a greater pressure; conversely, the smaller the sand ratio, the lower the slurry concentration, and thus it is easier to discharge the material, so the pressure of the pump truck when delivering the material is smaller.
[0110] When the pump truck is pumping the mixture, its feeding speed needs to be gradually increased until the filling speed reaches 2.8-4.2m 3 / min. In this process, the sand ratio also gradually increases. The purpose of this design is to prevent crack pressure from occurring due to excessive concentration of resin-coated sand and excessive pumping speed.
[0111] Comparative Example 10:
[0112] The difference between this comparative example and Example 1 is that the conveying pressure of the resin-coated sand is 65 MPa.
[0113] Comparative Example 11:
[0114] The difference between this comparative example and Example 1 is that the conveying pressure of the resin-coated sand is 70 MPa.
[0115]
[0116] After analysis, we found that due to the excessive delivery pressure in Comparative Examples 10 and 11, the resin-coated sand increased the crack thickness during the filling process, which in turn led to an increase in the amount of resin-coated sand and curing agent used.
[0117] Embodiment 5:
[0118] The difference between this embodiment and embodiment 1 is that, by weight, the ratio of the quartz sand, phenolic resin and coupling agent is 0.89:0.7:0.26; the ratio of the accelerator, pH regulator and polyol is 9.1:0.45:0.45.
[0119] The coupling agent is isopropyl tri(dioctyl pyrophosphate) titanate.
[0120] The accelerator is composed of formaldehyde and zinc chloride.
[0121] The pH adjuster is acetic acid.
[0122] The polyol is pentaerythritol.
[0123] Embodiment 6:
[0124] The difference between this embodiment and embodiment 1 is that, by weight, the ratio of the quartz sand, phenolic resin and coupling agent is 9:0.68:0.25; the ratio of the accelerator, pH regulator and polyol is 9.15:0.43:0.44.
[0125] The coupling agent is composed of a mixture of gamma-aminopropyltriethoxysilane and gamma-aminopropylmethyldiethoxysilane.
[0126] The accelerator consists of formaldehyde and copper sulfate.
[0127] The pH regulator is composed of a mixture of silicic acid and acetic acid.
[0128] The polyol is composed of a mixture of methyl propylene glycol and ethylene glycol.
[0129] Embodiment 7:
[0130] The difference between this embodiment and embodiment 1 is that, by weight, the ratio of the quartz sand, phenolic resin and coupling agent is 9.2:0.6:0.22; the ratio of the accelerator, pH regulator and polyol is 9.2:0.4:0.4.
[0131] The coupling agent is a mixture of monoalkoxy titanate, isopropyl tri(dioctyl pyrophosphate acyloxy) titanate, isopropyl dioleyl acyloxy (dioctyl phosphate acyloxy) titanate, γ-aminopropyl triethoxy silane and γ-aminopropyl methyl diethoxy silane.
[0132] The accelerator consists of formaldehyde, zinc chloride, copper sulfate and organic acid.
[0133] The pH regulator is composed of a mixture of citric acid, carbonic acid, silicic acid and acetic acid.
[0134] The polyol is composed of a mixture of pentaerythritol, glycerol, methyl propylene glycol, ethylene glycol, dipropylene glycol and neopentyl glycol.
[0135] In the four embodiments 1, 5, 6, and 7, the same filling parameters are used. The difference is that the composition ratios of the resin-coated sand and the curing agent in the four embodiments are different. The resin-coated sand and the curing agent in the embodiments 1, 5, 6, and 7 are respectively selected to carry out core strength simulation experiments, and the results are as follows:
[0136]
[0137] It can be seen from the core strength test in the above table that the materials provided by the above four embodiments all meet the national standards.
[0138] Comparative Example 12:
[0139] The difference between this comparative example and Example 1 is that, by weight, the usage ratio of the quartz sand, the phenolic resin and the coupling agent is 9.4:0.52:0.18.
[0140] Comparative Example 13:
[0141] The difference between this comparative example and Example 1 is that, by weight, the usage ratio of the quartz sand, the phenolic resin and the coupling agent is 8.5:0.8:0.2.
[0142] Comparative Example 14:
[0143] The difference between this comparative example and Example 1 is that, by weight, the usage ratio of the quartz sand, the phenolic resin and the coupling agent is 8.9:0.9:0.2.
[0144] Comparative Example 15:
[0145] The difference between this comparative example and Example 1 is that, by weight, the ratio of the accelerator, the pH adjuster and the polyol is 8.8:0.56:0.55.
[0146] Comparative Example 16:
[0147] The difference between this comparative example and Example 1 is that, by weight, the ratio of the accelerator, the pH adjuster and the polyol is 9.3:0.38:0.36.
[0148] Comparative Example 17:
[0149] The difference between this comparative example and Example 1 is that, by weight, the ratio of the accelerator, the pH adjuster and the polyol is 9.4:0.35:0.35.
[0150]
[0151] After analysis and comparison, we found that the lower core strength of Comparative Example 12 was due to the low surface coverage of quartz sand caused by the insufficient amount of phenolic resin.
[0152] Although the core strength of Comparative Example 13 is relatively high, the small amount of quartz sand used results in a waste of phenolic resin and thus increases the cost.
[0153] The lower core strength of Comparative Example 14 is due to the insufficient amount of coupling agent used, which results in the inability to fully cross-link and bond the quartz sand and the phenolic resin.
[0154] The lower core strength of Comparative Example 15 is due to the fact that too little accelerator is used, resulting in the inability of the resin-coated sand to be fully bonded together.
[0155] Although the core strength of Comparative Example 16 is relatively high, this is based on the simulated experimental environment without considering the alkaline environment.
[0156] The lower core strength of Comparative Example 17 is due to the fact that too little polyol is used, which results in the inability of the accelerator to fully catalyze, and thus the resin-coated sand cannot be fully bonded together.
[0157] Embodiment 8:
[0158] The difference between this embodiment and embodiment 1 is that the sand mixer needs to add phenolic resin powder when mixing high-purity quartz sand and phenolic resin solution. The weight ratio of phenolic resin solution to phenolic resin powder is 3.6:0.7.
[0159] Embodiment 9:
[0160] The difference between this embodiment and embodiment 1 is that the sand mixer needs to add phenolic resin powder when mixing high-purity quartz sand and phenolic resin solution. The weight ratio of phenolic resin solution to phenolic resin powder is 3.8:0.8.
[0161] Embodiment 10:
[0162] The difference between this embodiment and embodiment 1 is that the sand mixer needs to add phenolic resin powder when mixing high-purity quartz sand and phenolic resin solution. The weight ratio of phenolic resin solution to phenolic resin powder is 4.1:1.2.
[0163] Embodiment 11:
[0164] The difference between this embodiment and embodiment 1 is that the sand mixer needs to add phenolic resin powder when mixing high-purity quartz sand and phenolic resin solution. The weight ratio of phenolic resin solution to phenolic resin powder is 4.3:1.4.
[0165] Comparative Example 18:
[0166] The difference between this embodiment and embodiment 1 is that the sand mixer needs to add phenolic resin powder when mixing high-purity quartz sand and phenolic resin solution. The weight ratio of phenolic resin solution to phenolic resin powder is 3.6:0.5.
[0167] Comparative Example 19:
[0168] The difference between this embodiment and embodiment 1 is that the sand mixer needs to add phenolic resin powder when mixing high-purity quartz sand and phenolic resin solution. The weight ratio of phenolic resin solution to phenolic resin powder is 3.6:1.8.
[0169] The preliminary mixed materials in Example 1, Example 8-Example 11, Comparative Example 18-Comparative Example 19 were respectively sent to a vibrating air-cooling bed, and the wind speed of the vibrating air-cooling bed was 5000m 3 / h, working wind pressure is 1.6KPa, drying time is 30min, the results are as follows:
[0170]
[0171] It can be seen from the above table that the drying speed of the preliminary mixture is greatly increased in Examples 8 to 11 compared with Example 1. Although the drying speed of Comparative Examples 18 to 19 is poorer than that of Examples 8 to 11, the drying speed of Comparative Examples 18 to 19 is still higher than that of Example 1, which shows that the phenolic resin powder has a positive effect on promoting the drying speed of the resin-coated sand.
[0172] Embodiment 12:
[0173] The difference between this embodiment and embodiment 1 is that the concentration of the curing agent is 80%.
[0174] Embodiment 13:
[0175] The difference between this embodiment and embodiment 1 is that the concentration of the curing agent is 60%.
[0176] Comparative Example 20:
[0177] Randomly purchase three curing agents, o, p, and q, from the market.
[0178] The curing agent in Examples 1, 12, 13 and Comparative Example 20 was mixed with the resin-coated sand. The relationship between the curing time and the temperature of the resin-coated sand is shown in the following table:
[0179]
[0180] It can be seen from the above table that as the temperature rises, the concentration of the curing agent gradually decreases, but the solidification time gradually becomes the same. Therefore, the curing agent of appropriate concentration can be prepared according to the temperature of the oil well fracture to reduce costs.
[0181] By comparing o, p, q with the curing agent in this scheme, it can be seen that the curing agent in this scheme can still catalyze the resin-coated sand for consolidation under low temperature environment, but o will not consolidate at 20-40°C, and p and q will not consolidate at 20-30°C.
[0182] From the above table, we can infer that the concentration of the curing agent in the mixed solution changes with temperature. The calculation formula for the curing agent concentration is:
[0183] ,
[0184] b is the concentration of curing agent, a is the temperature at the oil well fracture (℃), a≥55℃.
[0185] In this scheme, 55℃ is the starting temperature. It can be seen from the above formula that when the temperature exceeds 55℃, the curing agent concentration should decrease by 20% for every 10℃ increase. When the oil well fracture concentration is lower than 55℃, in order to ensure the consolidation efficiency, the amount of water in the mixed solution of curing agent and water is 0, that is, the concentration of curing agent is 100%.
[0186] To sum up, this scheme has the following advantages: First, it uses high-quality quartz sand as raw material, which can adapt to the fracturing and sand control construction needs of different depth formations; second, the resin-coated sand has high bonding strength after curing and is not easy to be damaged; third, the construction process is not affected by the number of layers, thickness, and span of the construction well; fourth, it has strong adaptability to the bonding and curing environment, can adapt to the sand control needs at different temperatures, and solves the problem of difficult bonding and curing at low temperatures; fifth, it has a wide range of applications and can be applied to vertical, inclined, horizontal wells and window side drilling; sixth, the resin-coated sand after bonding has excellent chemical stability, corrosion resistance, and high structural strength.
[0187] The present invention is not limited to the above-mentioned specific implementation modes. Various changes made by ordinary technicians in this field based on the above-mentioned concepts without creative work are all within the protection scope of the present invention.
Claims
1. A sand control method for fracturing tail chasing, characterized in that: The following steps are involved: Step 1, preparing resin-coated sand; The high-purity quartz sand and the phenolic resin solution are sent to a sand mixer for mixing, a coupling agent is added during the mixing process, and a preliminary mixture is obtained after the mixing is completed; the preliminary mixture is sent to a disperser through a conveyor belt for dispersion, and the dispersed preliminary mixture is sent to a vibrating air-cooled bed for drying to obtain resin-coated sand; Step 2, preparing a curing agent; The accelerator, pH adjuster and polyol are sent to a mixing kettle for stirring and mixing to obtain a curing agent; Step 3, crack filling; First, high-purity quartz sand is mixed with sand-carrying fluid and then pumped to the cracks of the oil well by a fracturing pump truck, and the high-purity quartz sand is mixed with the original formation to form a mixed sand zone; secondly, the resin-coated sand in step 1 is pumped to the cracks of the oil well by a fracturing pump truck, and then the curing agent in step 2 is sent to the cracks of the oil well by a fracturing pump truck, and the curing agent moves toward the mixed sand zone through the gaps between the resin-coated sands. In this process, the curing agent catalyzes the bonding of the resin-coated sand to form a support zone; finally, the curing agent catalyzes the bonding of the resin-coated sand in the perforated blasthole to form a leakage zone; In step 3, the curing agent is mixed with water and then delivered to the crack of the oil well by a fracturing pump truck; the curing agent is mixed with water to obtain a mixed solution, and the concentration of the curing agent in the mixed solution changes with temperature. The calculation formula of the curing agent concentration is: , b is the concentration of curing agent, a is the temperature at the oil well fracture, ℃, a≥55℃; In step 1, the sand mixer also needs to add phenolic resin powder when mixing high-purity quartz sand and phenolic resin solution, and the weight ratio of phenolic resin solution to phenolic resin powder is 3.6-4.3:0.7-1.4; The coupling agent is composed of one or more of monoalkoxy titanate, γ-aminopropyl triethoxy silane, and γ-aminopropyl methyl diethoxy silane; the accelerator is one or more of formaldehyde, zinc chloride, copper sulfate, and organic acid; the pH regulator is composed of one or more of citric acid, carbonic acid, silicic acid, and acetic acid; and the polyol is composed of one or more of pentaerythritol, glycerol, methyl propylene glycol, ethylene glycol, dipropylene glycol, and neopentyl glycol.
2. The sand control method for fracturing tailing according to claim 1, characterized in that: In the resin coated sand, the resin coating rate on the surface of the quartz sand is ≥97%.
3. The sand control method for fracturing tailing according to claim 1, characterized in that: The particle size of the resin coated sand is 0.3-1.4 mm, the particle dispersion rate of the resin coated sand is ≥98%, and the density of the resin coated sand is 1.3-1.6 t / m 3 .
4. The sand control method for fracturing tailing according to claim 1, characterized in that: Calculated by usage volume, the usage ratio of the resin-coated sand to the curing agent is 1-1.2:0.8-1.
5. The sand control method for fracturing tailing according to claim 1, characterized in that: At 20°C, the acidity of the curing agent is 0.3-0.6 mol / L, and the density of the curing agent is 0.9 t / m 3 -1.1t / m 3 .
6. The sand control method for fracturing tailing according to claim 1, characterized in that: In step 3, the resin-coated sand is mixed with the sand-carrying fluid and then pumped to the oil well fracture by a fracturing pump truck. The filling speed of the resin-coated sand and sand-carrying fluid mixture is 2.8-4.2 m / s. 3 / min, the conveying pressure of the resin-coated sand is ≤60MPa.