Method for reducing corrosion of nickel smelting flue gas acid making absorption tower bottom return acid to circulating tank
By controlling the flue gas pressure of the acid-making system, adjusting the process parameters of the Australian furnace, and setting up negative pressure pipelines, the problem of corrosion of the circulation tank during the acid-making process of nickel smelting flue gas was solved, and stable operation of the equipment and improvement of production efficiency were achieved.
Patent Information
- Application Number
- CN202410817341.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-01
AI Technical Summary
In the acid production process from nickel smelting flue gas, the discontinuous production of the converter causes large pressure fluctuations in the flue gas system and changes in CO and NOx concentrations, causing blockage of the absorption tower and corrosion of the circulation tank, increasing equipment failure rates and affecting production efficiency and costs.
By controlling the flue gas pressure of the acid-making system, adjusting the process parameters of the Australian furnace, setting up negative pressure pipelines, adjusting the acid distributor and temperature of the absorption tower, ensuring a slight negative pressure inside the circulation tank, reducing the entry of high-temperature corrosive gases, and stabilizing the operation of the acid-making system .
It reduces circulation tank corrosion failures, improves production continuity and efficiency, reduces production costs, and extends equipment service life.
Smart Images

Figure CN118718672A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of acid production from flue gas of nickel smelting, and in particular to a method for reducing the corrosion of a circulation tank by acid return at the bottom of an absorption tower of nickel smelting flue gas acid production. Background Art
[0002] This flue gas acid production project adopts the advanced technology and mature experience of dynamic wave dilute acid washing purification, 3+1 four-stage conversion, and double absorption acid production process. During the acid production process, it mainly receives the Australian furnace smelting flue gas and converter blowing flue gas. However, due to the non-continuous production of the converter during the production process, the pressure changes in the flue gas system fluctuate greatly. At the same time, the amount of materials added to the Australian furnace, the composition of the flue gas, and the changes in the reaction atmosphere in the furnace will cause the acid production to be uncontrollable. CO and NO will be generated during the production process. x The former causes a sudden rise in the temperature of the acid conversion system, requiring a large amount of air to purge and cool down. The latter causes dry absorption of sulfuric acid to produce nitrosylsulfuric acid, causing crystallization and blockage of the fiber demister on the upper part of the absorption tower, poor flue gas flow, and excessive pressure inside the absorption tower and circulation tank. In addition, because the design structure of the circulation tank is acid return on the tower wall, it cannot form a liquid seal when the amount of circulating acid is certain, resulting in a large amount of high-temperature flue gas entering the circulation tank, which increases the corrosion failure rate of the equipment. Summary of the invention
[0003] The purpose of the present invention is to overcome the defects of the prior art and propose a method for reducing the corrosion of the circulation tank by the acid return at the bottom of the nickel smelting flue gas acid-making absorption tower, which can reduce the number of production stoppages caused by equipment failure due to corrosion of the circulation tank, improve production efficiency and reduce production costs.
[0004] To achieve the above object, the present invention adopts the following specific technical solutions:
[0005] The method provided by the present invention for reducing the corrosion of the circulation tank by the acid return at the bottom of the nickel smelting flue gas acid-making absorption tower comprises the following steps:
[0006] Step 1: Control the flue gas pressure of the acid production system; the smelting flue gas is discharged into the main flue through the exhaust fan after being dedusted by the electric dust collector. 2 The relay fan enters the acid making system to ensure that there is no cross-fire at the charging port of the Australian furnace;
[0007] Step 2: Adjust the furnace process parameters; by adjusting the feed amount, exhaust fan speed, air volume, fuel, oxidation and reduction atmosphere inside the furnace, reduce the flue gas system pressure fluctuation to control CO, NO x The concentration of acid can ensure the stable operation of the acid making system;
[0008] Step 3, set up a negative pressure pipeline; set up negative pressure pipelines connected to the inlet of the drying tower at the overflow pipelines of the first circulation tank and the second circulation tank respectively, so that a slight negative pressure is formed inside the first circulation tank and the second circulation tank, which is used to reduce the corrosion of the circulation tank and the circulation pump caused by the positive pressure generated by the high-temperature corrosive gas entering the first circulation tank and the second circulation tank;
[0009] Step 4: Adjust the acid distributors in the first absorption tower and the second absorption tower to control the amount of circulating acid, and adjust the temperature and pressure of the first absorption tower and the second absorption tower to control the concentration of absorbed acid.
[0010] Preferably, in step 1, the flue gas pressure of the acid-making system is controlled at -0.6 kPa to -1.0 kPa.
[0011] Preferably, in step 2, the concentration of CO is controlled to be less than 800 ppm to prevent the temperature of the acid conversion system from being too high; x Concentration <400 mg / m 3 , to prevent the formation of nitrosylsulfuric acid in the first absorption tower and the second absorption tower, and to block the fiber demister in the absorption tower to increase the pressure in the absorption tower.
[0012] Preferably, in step 4, the temperatures of the first absorption tower and the second absorption tower are 75° C. and 70° C. respectively, the upper pressures of the first absorption tower and the second absorption tower are 0.181 MPa and 0.176 MPa respectively, and the absorbed acid concentration is 98.3% to 98.8%.
[0013] The present invention can achieve the following technical effects:
[0014] The present invention achieves stable operation of the converter and the acid-making system by controlling the flue gas system pressure to be stable; by adding a tee at the overflow port of the two absorption circulation tanks to retain the existing overflow effect, the other end is introduced into the drying tower inlet through a pipeline to ensure the slight negative pressure operation inside the circulation tank, reduce the corrosion failure rate of the equipment, meet the continuous and stable production requirements, improve production efficiency and reduce production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a schematic diagram of the overall process of the method of the present invention. DETAILED DESCRIPTION
[0016] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. In the following description, the same modules are represented by the same reference numerals. In the case of the same reference numerals, their names and functions are also the same. Therefore, the detailed description thereof will not be repeated.
[0017] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and do not constitute a limitation of the present invention.
[0018] The embodiment of the present invention provides a method for reducing the corrosion of the circulating tank by the acid return at the bottom of the nickel smelting flue gas acid-making absorption tower. The overall process is as follows: Figure 1 As shown, including:
[0019] Step 1: Control the flue gas pressure of the acid production system; the smelting flue gas is discharged into the main flue through the exhaust fan after being dedusted by the electric dust collector. 2 The relay fan enters the acid making system to ensure that there is no cross-fire at the charging port of the Australian furnace;
[0020] Step 2: Adjust the furnace process parameters; by adjusting the feed amount, exhaust fan speed, air volume, fuel, oxidation and reduction atmosphere inside the furnace, reduce the flue gas system pressure fluctuation to control CO, NO x The concentration of acid can ensure the stable operation of the acid making system;
[0021] Step 3, set up a negative pressure pipeline; set up negative pressure pipelines connected to the inlet of the drying tower at the overflow pipelines of the first circulation tank and the second circulation tank respectively, so that a slight negative pressure is formed inside the first circulation tank and the second circulation tank, which is used to reduce the corrosion of the circulation tank and the circulation pump caused by the positive pressure generated by the high-temperature corrosive gas entering the first circulation tank and the second circulation tank;
[0022] Step 4: Adjust the acid distributors in the first absorption tower and the second absorption tower to control the amount of circulating acid, and adjust the temperature and pressure of the first absorption tower and the second absorption tower to control the concentration of absorbed acid.
[0023] The following describes the invention in conjunction with specific embodiments.
[0024] Example 1
[0025] Step 1: Control the flue gas pressure of the acid-making system. When the Australian furnace and the converter are in production at the same time, the inlet pressure of the acid-making purification is controlled at -1.0kpa to ensure that there is no cross-fire at the Australian furnace intersection and no smoke from the converter hood. When the converter is waiting for feeding and the air is not turned on, the inlet pressure is controlled at -0.6kpa.
[0026] Step 2: Adjust the process parameters of the Australian furnace; the main control personnel control various parameters and at the same time convert the CO and NO fed back by the sulfuric acid inlet analyzer. x Adjust parameters in time to ensure stable operation of the acid making system.
[0027] Step 3: Negative pressure pipeline operation. The valve at the entrance of the drying tower should be fine-tuned in time according to the pressure conditions to avoid excessive negative pressure that will draw in acid mist and corrode the flue, and to avoid excessive negative pressure that will cause positive pressure operation in the circulation tank and corrode the circulation tank equipment.
[0028] Step 4: Control the circulating acid amount. Operate according to the circulating acid amount and Hz data of the circulating pump debugged before the system starts. At the same time, the laboratory regularly tests the absorption efficiency. According to the test data, the circulating acid amount is adjusted in time to achieve the best absorption effect and no excessive flue gas enters the circulation tank;
[0029] Strictly control the acid concentration and acid temperature, stabilize the absorption acid concentration at 98.3% to 98.8%, and avoid the formation of fuming acid due to excessive concentration. Strictly control the first absorption temperature at 75℃ and the second absorption temperature at 70℃, and avoid the formation of acid mist and increased corrosion rate due to excessive temperature.
[0030] Example 2
[0031] Step 1. Control the flue gas pressure of the acid-making system; Reasonably control the flue gas pressure of the acid-making system. When the Australian furnace and the converter are in production at the same time, the acid purification inlet pressure is controlled at -1.0kpa to ensure that there is no cross-fire at the Australian furnace intersection and no smoke from the converter hood. When the converter is waiting for feeding and the air is not turned on, the inlet pressure is controlled at -0.6kpa.
[0032] Step 2: Adjust the process parameters of the Australian furnace; the main control personnel control various parameters and at the same time convert the CO and NO fed back by the sulfuric acid inlet analyzer. x Adjust the parameters in time to ensure the stable operation of the acid production system. If it cannot be controlled for a long time, the Australian furnace should reduce the amount of material and notify the Australian furnace to resume normal operation after the system stabilizes.
[0033] Step three: negative pressure pipeline operation. The valve at the entrance of the drying tower should be fine-tuned in time according to the pressure conditions to avoid excessive negative pressure that will draw in acid mist and corrode the flue, and to avoid excessive negative pressure that will cause positive pressure operation in the circulation tank and corrode the circulation tank equipment. At the same time, during the inspection, the personnel will touch the temperature of the negative pressure of the two circulation tank branches with their hands to determine whether a certain circulation tank is unobstructed and whether a liquid seal is formed at the overflow port due to excessively high liquid level.
[0034] Step 4: Control the circulating acid amount. Operate according to the circulating acid amount and Hz data of the circulating pump debugged before the system starts. At the same time, the laboratory regularly tests the absorption efficiency. According to the test data, the circulating acid amount is adjusted in time to achieve the best absorption effect and no excessive flue gas enters the circulation tank;
[0035] Strictly control the acid concentration and acid temperature, stabilize the absorption acid concentration at 98.3%-98.8%, and avoid the formation of fuming acid due to excessive concentration. Strictly control the first absorption temperature at 75℃ and the second absorption temperature at 70℃ to avoid the formation of acid mist and increased corrosion rate due to excessive temperature. If the acid concentration is too high, add water to dilute it to the index requirements in time. If the acid temperature is too high, adjust it to the index requirements through acid stringing in time;
[0036] The method of the present invention controls the inlet pressure of the acid purification system to operate between -0.6 kpa and -1.0 kpa, and the valve opening of the negative pressure pipeline of the circulation tank is adjusted in time according to the pressure conditions to ensure that the circulation tank operates under a slight negative pressure state.
[0037] The negative pressure pipeline of the present invention is made of steel-lined polytetrafluoroethylene material, the two circulation tank branch pipelines are DN150, the drying tower inlet main line is DN250, and there are three sets of corresponding polytetrafluoroethylene-lined valves. The system operates continuously during production, and the inside of the circulation tank changes from a positive pressure state to a slightly negative pressure state, which not only plays a role in the corrosion protection of the equipment, but also greatly improves the internal environment of the factory building.
[0038] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0039] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
[0040] The above specific implementations of the present invention do not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for reducing the corrosion of the circulation tank by the acid return at the bottom of the nickel smelting flue gas acid-making absorption tower, characterized in that: The steps include: Step 1: Control the flue gas pressure of the acid-making system; the smelting flue gas is discharged into the main flue by the exhaust fan after being dedusted by the electric dust collector, and enters the acid-making system through the SO2 relay fan to ensure that there is no cross-fire at the charging port of the Australian furnace; Step 2: Adjust the furnace process parameters; by adjusting the feed amount, exhaust fan speed, air volume, fuel, oxidation and reduction atmosphere inside the furnace, reduce the flue gas system pressure fluctuation to control CO, NO x The concentration of acid can ensure the stable operation of the acid making system; Step 3, set up a negative pressure pipeline; set up negative pressure pipelines connected to the inlet of the drying tower at the overflow pipelines of the first circulation tank and the second circulation tank respectively, so that a slight negative pressure is formed inside the first circulation tank and the second circulation tank, which is used to reduce the corrosion of the circulation tank and the circulation pump caused by the positive pressure generated by the high-temperature corrosive gas entering the first circulation tank and the second circulation tank; Step 4: Adjust the acid distributors in the first absorption tower and the second absorption tower to control the amount of circulating acid, and adjust the temperature and pressure of the first absorption tower and the second absorption tower to control the concentration of absorbed acid.
2. The method for reducing the corrosion of the circulation tank by the acid return at the bottom of the nickel smelting flue gas acid-making absorption tower according to claim 1, characterized in that: In step 1, the flue gas pressure of the acid-making system is controlled at -0.6 kPa to -1.0 kPa.
3. The method for reducing the corrosion of the circulation tank by the acid return at the bottom of the nickel smelting flue gas acid-making absorption tower according to claim 1, characterized in that: In step 2, the concentration of CO is controlled to be less than 800ppm to prevent the temperature of the acid conversion system from being too high; x Concentration <400 mg / m 3 , to prevent the formation of nitrosylsulfuric acid in the first absorption tower and the second absorption tower, and to block the fiber demister in the absorption tower to increase the pressure in the absorption tower.
4. The method for reducing the corrosion of the circulation tank by the acid return at the bottom of the nickel smelting flue gas acid-making absorption tower according to claim 1, characterized in that: In step 4, the temperatures of the first absorption tower and the second absorption tower are 75° C. and 70° C. respectively, the upper pressures of the first absorption tower and the second absorption tower are 0.181 MPa and 0.176 MPa respectively, and the absorbed acid concentration is 98.3% to 98.8%.