Graphene heat-conducting film coiled material and preparation method thereof

Through the steps of preparation, winding, pretreatment and graphitization, the preparation process of graphene thermal conductive film is optimized, which solves the problems of low efficiency of traditional process and film expansion and blistering, and achieves graphene with higher thickness and higher thermal conductivity. Thermal conductive film roll.

CN118723980APending Publication Date: 2024-10-01XINGTU (CHANGZHOU) CARBON MATERIALS CO LTD

Patent Information

Application Number
CN202311806384.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The traditional graphene thermal conductive film preparation process is inefficient and cannot meet the needs of industrial continuous production. The breakage of gas and heat during the heat treatment of graphene oxide causes the film to expand, bubble and crack, which limits the thermal conductivity performance and scope of use.

Method used

The steps of preparation, slitting, winding, pretreatment, graphitization and calendering of graphene oxide diaphragms are adopted. Through gradient heating and optimization of squeeze roller pressure, the tightness of the diaphragm and the pretreatment temperature gradient are controlled to ensure that the gas and Proper heat dissipation prevents film decomposition and improves the orderly rearrangement of carbon elements.

Benefits of technology

It significantly improves the thickness and thermal conductivity of the graphene thermally conductive film, solves the problems of film unevenness, explosion and cracking, improves the production yield and thermal conductivity, and enables the preparation of higher thickness graphene coils.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004630383370000011
    Figure HDA0004630383370000011
  • Figure HDA0004630383370000012
    Figure HDA0004630383370000012
  • Figure HDA0004630383370000021
    Figure HDA0004630383370000021
Patent Text Reader

Abstract

The invention relates to the field of C01B32 / 154, and particularly provides a graphene heat-conducting film coiled material and a preparation method thereof. The preparation method sequentially comprises the following steps: preparation of a graphene oxide membrane, stripping, winding, pretreatment, graphitization treatment, calendering and lamination. The pretreatment comprises the following steps of: performing heat treatment on the coiled material in a gradient heating program; the gradient heating temperature ranges from 25 DEG C to 350 DEG C, and the treatment time ranges from 30 h to 120 h; the tightness of the diaphragm in the winding step is 10-100%; the graphitization process is optimized; not only are the product yield and the heat conductivity effectively improved, but also the thickness of the heat conducting film in the coiled material can reach up to 200 microns.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of graphene thermal conductive films, C01B32 / 154, and in particular to a graphene thermal conductive film coil and a preparation method thereof. Background Art

[0002] Graphene thermal conductive film is widely used in electronics, communications, aviation, national defense and military industries due to its high thermal conductivity, light weight and small size. In the traditional preparation process, graphite paper and graphene oxide film are generally stacked layer by layer for heat treatment, which has low production capacity and low efficiency; most existing processes use coating heat treatment method, which is not continuous and can only prepare graphene sheets, which not only cannot meet the production needs of industrial automation, but also limits its scope of use.

[0003] Some technologies have focused on the preparation of graphene rolls in order to seek continuous industrial use. However, the structure of the raw material graphene oxide contains a large number of oxygen-containing functional groups. During the heat treatment process, the fracture and decomposition of these functional groups will produce a large amount of gas and heat, leading to volume expansion, blistering and cracking of the film, resulting in product scrapping or a serious decrease in thermal conductivity.

[0004] Chinese patent CN113480328A discloses a large-scale graphene thermal conductive roll film and its preparation method. The patent introduces fiber fabrics and nanocellulose to establish exhaust channels in the film, promotes the discharge of gas, heat, etc. during the heat treatment process, and improves the production yield of the thermal roll film. Chinese patent CN114590803A discloses a manufacturing process for graphene heat dissipation film coils. The patent facilitates the discharge of gases such as water and carbon dioxide during high-temperature processes by controlling the winding speed and tension, low-temperature treatment temperature and duration, and punching holes on the graphene film to improve the yield of the graphene coil. However, the processes of the above patents are relatively cumbersome, and the maximum thickness of the produced coil film is only 25μm, which greatly limits the scope of use and performance of the graphene thermal conductive film. Summary of the invention

[0005] In order to solve the above technical problems, the present invention first provides a method for preparing a graphene thermal conductive film coil.

[0006] Furthermore, the preparation method comprises the following steps in sequence: graphene oxide membrane preparation, striping, winding, pretreatment, graphitization treatment, calendering, and bonding.

[0007] Furthermore, the preparation steps of the graphene oxide membrane are as follows: (1) mixing graphene oxide and water, dispersing them evenly, and then homogenizing and degassing them to obtain a slurry; (2) coating the slurry on a circulating substrate through a coater, and the coating wet film thickness is 2.0 mm-6.0 mm; (3) setting the coating machine tunnel temperature to 65-90°C, drying at a drying speed of 0.2-1.5 m / min, and after drying, peeling the graphene oxide film from the substrate and rolling it up.

[0008] Furthermore, in the step (1), the solid content of the graphene oxide and water after mixing is 2-15%, preferably 3-10%, and more preferably 3-8%.

[0009] Furthermore, the present invention does not impose strict requirements on the dispersion form of step (1), as long as the dispersion is uniform.

[0010] Preferably, the dispersion in step (1) is carried out by stirring in a mixer at a rotation speed of 200-600 rpm for 20-60 min, and then stirring at a rotation speed of 700-1200 rpm for 10-60 min.

[0011] Furthermore, the width of the recycled substrate is 100-200 cm.

[0012] Furthermore, the winding step of the graphene oxide is: placing the graphene oxide membrane on a unwinding shaft, placing the graphite tube core on a reeling shaft, and evenly winding the membrane onto the graphite tube core by rotating the unwinding and reeling shafts, and controlling the tightness of the membrane to be 10-100%, preferably 20-100%.

[0013] Furthermore, the calculation formula of the tightness is: tightness=[diaphragm length×diaphragm thickness] / [large roll area-tube core area].

[0014] More preferably, the tightness of the diaphragm is 40-90%.

[0015] Furthermore, the pretreatment step is: placing the coiled material in a gradient heating program for heat treatment; the gradient heating temperature is 25-350° C., and the treatment time is 30-120 hours.

[0016] Furthermore, the gradient heating temperature is: 75-85°C for 3-25h, 90-120°C for 3-25h, 130-170°C for 3-25h, 180-220°C for 3-25h, 230-270°C for 3-25h, and 280-330°C for 3-25h.

[0017] The graphene oxide film will expand during the high temperature treatment process, and will release heat and a large amount of gas. Through the loose coiling process, the adjacent film layers of the graphene oxide film loose coil have a suitable gap, which is convenient for the volatilization and discharge of water vapor, oxygen and other gases and heat during the heat treatment. The present invention stipulates that the tightness = film length * film thickness / (large roll area - tube core area), which can preliminarily solve the problem that the graphene coil with higher thickness is prone to uneven film, explosion and cracking. In addition, the heating temperature and treatment time of the pretreatment operation are stipulated to eliminate the adsorbed water in the graphene oxide film, and make most of the oxygen-containing functional groups such as -COC-, -COOH, -OH, etc. decompose at a suitable speed, which can not only further flatten the film surface, but also prevent the explosion of the furnace caused by a large amount of decomposed gas and heat in the later high temperature protection process (carbonization, graphitization process).

[0018] Preferably, the gradient heating temperature is: heating from room temperature to 80°C for 0.5-1.5h, then maintaining at 80°C for 4-22h, 90-110°C for 4-22h, 140-160°C for 4-22h, 190-210°C for 4-22h, 240-260°C for 4-22h, and 290-310°C for 4-22h.

[0019] More preferably, the gradient heating temperature is: heating from room temperature to 80°C for 1 hour, then maintaining at 80°C for 5-20 hours, 100°C for 5-20 hours, 150°C for 5-20 hours, 200°C for 5-20 hours, 250°C for 5-20 hours, and 300°C for 5-20 hours.

[0020] Furthermore, the temperature of the graphitization treatment step is 1000-3500° C., and the firing time is 5-40 hours.

[0021] Preferably, the graphitization treatment step is: the pretreated membrane is placed in a graphite furnace and a protective gas is introduced for high-temperature firing, and the temperature curve is set as follows: heating from room temperature to 1000°C for 6-15 hours; maintaining at 1000-1500°C for 2-10 hours; maintaining at 1500-2000°C for 3-10 hours; maintaining at 2000-3000°C for 3-10 hours; and finally maintaining at 3000-3500°C for 1-4 hours. This process realizes the rearrangement of carbon element molecules, transforming from disorder to order, and improving its thermal conductivity.

[0022] Further preferably, the graphitization treatment step is: the pretreated membrane is placed in a graphite furnace and a protective gas is introduced for high-temperature firing, and the temperature curve is set as: heating from room temperature to 1000°C for 8-11 hours; maintaining at 1000-1500°C for 4-6 hours; maintaining at 1500-2000°C for 5-8 hours; maintaining at 2000-3000°C for 3-5 hours; and finally keeping at 3000-3500°C for 1-3 hours.

[0023] Furthermore, the protective gas includes but is not limited to at least one of argon, nitrogen, helium and hydrogen.

[0024] Preferably, the protective gas comprises argon.

[0025] Furthermore, the calendering step uses an extrusion roller to extrude the coil, and the pressure of the extrusion roller is 2-5 T. Rolling can increase the density of the graphene heat dissipation coil and improve the thermal conductivity, but too high rolling pressure will not only cause adhesion between graphene film layers and affect its thermal conductivity, but may also cause the film fracture length to decrease.

[0026] Furthermore, the laminating step is to laminate the film onto the substrate, which is convenient for the subsequent die-cutting process.

[0027] Secondly, the present application also provides a graphene thermally conductive film coil prepared according to the preparation method; the thickness of the graphene thermally conductive film is 5-200 μm, preferably 10-200 μm.

[0028] Beneficial Effects

[0029] 1. This application optimizes the winding tightness according to the thickness of the thermal conductive film, and further selects the temperature gradient program of the pretreatment, so that part of the gas and heat in the film are discharged at a suitable speed without affecting the flatness of the film surface, which can improve the production yield and increase the thickness of the film;

[0030] 2. This application further optimizes the temperature and processing time of the graphitization process, effectively avoiding technical problems such as film blistering and film cracking caused by the precipitation of gas and heat, and makes the rearrangement of carbon elements in the film reach the optimal state, further improving the thickness and thermal conductivity of the thermal conductive film;

[0031] 3. The thickness of the thermal conductive film in the coil of the present application is 20-100 μm, which achieves a significant increase in thickness compared to the 20 μm thick film layer in the industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 : Scanning electron microscope image of the graphene thermal conductive film coil of Example 1 (size specification: 50 μm);

[0033] Figure 2 : Scanning electron microscope image of the graphene thermal conductive film coil of Example 1 (size specification: 20 μm);

[0034] Figure 3 : Scanning electron microscope image of the graphene thermal conductive film coil of Comparative Example 1 (size specification: 10 μm);

[0035] Figure 4: Scanning electron microscope image of the graphene thermal conductive film coil of Comparative Example 1 (size specification: 5 μm);

[0036] Figure 5 : Thermogravimetric curve of the graphene thermal conductive film of Example 1;

[0037] Figure 6 : Thermogravimetric curve of the graphene thermal conductive film of Example 3;

[0038] Figure 7 : Physical picture of the graphene thermal conductive film coil of Example 1 (specification: 1000m length);

[0039] Figure 8 : Actual pictures of graphene thermal conductive film rolls of different specifications in Example 1. DETAILED DESCRIPTION

[0040] Example

[0041] Example 1

[0042] This embodiment provides a method for preparing a graphene thermal conductive film coil, which comprises the following steps in sequence:

[0043] (1) Preparation of graphene oxide membrane: Graphene oxide and water were mixed to ensure that the solid content of the solution was 3%. The mixture was stirred in a mixer at a speed of 400 rpm for 30 min and then at a speed of 900 rpm for 30 min. After uniform dispersion, the mixture was homogenized and degassed to obtain a slurry. The slurry was coated on a circulating substrate (with a width of 200 cm) by a coater to a wet film thickness of 2.0 mm. The tunnel temperature of the coater was set at 80° C. and the mixture was dried at a drying speed of 1.0 m / min. After drying, the graphene oxide membrane was peeled off from the substrate and rolled up.

[0044] (2) Striping;

[0045] (3) Winding: Place the graphene oxide membrane on the unwinding shaft and the graphite tube core on the winding shaft. By rotating the unwinding and winding shafts, the membrane is evenly wound onto the graphite tube core, and the tightness of the membrane is controlled to be 20%. The calculation formula for the tightness is: tightness = [membrane length × membrane thickness] / [large roll area - tube core area].

[0046] (4) Pretreatment: The coiled material is placed in a gradient heating program for heat treatment, wherein the gradient heating temperature is: room temperature to 80°C for 1 hour, then maintained at 80°C for 12 hours, 100°C for 12 hours, 150°C for 12 hours, 200°C for 12 hours, 250°C for 12 hours, and 300°C for 12 hours.

[0047] (5) Graphitization treatment: The pretreated membrane is placed in a graphite furnace and argon gas is introduced for high-temperature firing. The temperature curve is set as follows: from room temperature to 1000°C for 10 hours; maintained at 1300°C for 5 hours; maintained at 1800°C for 6 hours; maintained at 2500°C for 4 hours; and finally maintained at 3200°C for 1 hour.

[0048] (6) Calendering: The coil is extruded by an extrusion roller, and the pressure of the extrusion roller is 4T.

[0049] (7) Bonding: Bond the obtained film onto the PET film.

[0050] The graphene thermally conductive film of the graphene thermally conductive film coil of the present embodiment has a thickness of 10 μm, a width of 150±5 mm, a length of 100-110 m, a thermal conductivity of 1900 W / mk, and a smooth film surface without bubbling or cracking.

[0051] Example 2

[0052] This embodiment provides a method for preparing a graphene thermal conductive film coil, which comprises the following steps in sequence:

[0053] (1) Preparation of graphene oxide membrane: Graphene oxide and water were mixed to ensure that the solid content of the solution was 5%, and the mixture was stirred in a mixer at a speed of 200 rpm for 60 min, and then at a speed of 1200 rpm for 10 min. After being evenly dispersed, the mixture was homogenized and degassed to obtain a slurry. The slurry was coated on a circulating substrate (with a width of 200 cm) by a coater, and the coating wet film thickness was 3.0 mm. The coating tunnel temperature was set to 65° C., and the mixture was dried at a drying speed of 0.2 m / min. After drying, the graphene oxide membrane was peeled off from the substrate and rolled up.

[0054] (2) Striping;

[0055] (3) Winding: Place the graphene oxide membrane on the unwinding shaft and the graphite tube core on the winding shaft. By rotating the unwinding and winding shafts, the membrane is evenly wound onto the graphite tube core, and the tightness of the membrane is controlled to be 40%. The calculation formula for the tightness is: tightness = [membrane length × membrane thickness] / [large roll area - tube core area].

[0056] (4) Pretreatment: The coiled material is placed in a gradient heating program for heat treatment, wherein the gradient heating temperature is: room temperature to 80°C for 1 hour, then maintained at 80°C for 20 hours, 100°C for 20 hours, 150°C for 20 hours, 200°C for 20 hours, 250°C for 5 hours, and 300°C for 5 hours.

[0057] (5) Graphitization treatment: The pretreated membrane is placed in a graphite furnace and argon gas is introduced for high-temperature firing. The temperature curve is set as follows: heating from room temperature to 1000°C for 8 hours; maintaining at 1000°C for 6 hours; maintaining at 1500°C for 8 hours; maintaining at 2000°C for 5 hours; and finally maintaining at 3000°C for 2 hours.

[0058] (6) Calendering: The coil is extruded by an extrusion roller, and the pressure of the extrusion roller is 5T.

[0059] (7) Bonding: Bond the obtained film onto the PET film.

[0060] The graphene thermally conductive film of the graphene thermally conductive film coil of the present embodiment has a thickness of 25 μm, a width of 150±5 mm, a length of 100-110 m, a thermal conductivity of 1600 W / mk, and a smooth film surface without bubbling or cracking.

[0061] Example 3

[0062] This embodiment provides a method for preparing a graphene thermal conductive film coil, which comprises the following steps in sequence:

[0063] (1) Preparation of graphene oxide membrane: Graphene oxide and water were mixed to ensure that the solid content of the solution was 6%, and the mixture was stirred in a blender at a speed of 600 rpm for 20 min and then at a speed of 700 rpm for 60 min. After being evenly dispersed, the mixture was homogenized and degassed to obtain a slurry. The slurry was coated on a circulating substrate (with a width of 100 cm) by a coater to a wet film thickness of 4.0 mm. The coating tunnel temperature of the coater was set at 90° C. and the mixture was dried at a drying speed of 1.5 m / min. After drying, the graphene oxide membrane was peeled off from the substrate and rolled up.

[0064] (2) Striping;

[0065] (3) Winding: Place the graphene oxide membrane on the unwinding shaft and the graphite tube core on the winding shaft. By rotating the unwinding and winding shafts, the membrane is evenly wound onto the graphite tube core, and the tightness of the membrane is controlled to be 60%. The calculation formula for the tightness is: tightness = [membrane length × membrane thickness] / [large roll area - tube core area].

[0066] (4) Pretreatment: The coiled material is placed in a gradient heating program for heat treatment, wherein the gradient heating temperature is: room temperature to 80°C for 1 hour, then maintained at 80°C for 10 hours, 100°C for 15 hours, 150°C for 15 hours, 200°C for 15 hours, 250°C for 15 hours, and 300°C for 15 hours.

[0067] (5) Graphitization treatment: The pretreated membrane is placed in a graphite furnace and argon gas is introduced for high-temperature firing. The temperature curve is set as follows: from room temperature to 1000°C for 8 hours; maintained at 1500°C for 4 hours; maintained at 2000°C for 8 hours; maintained at 2500°C for 3 hours; and finally maintained at 2800°C for 3 hours.

[0068] (6) Calendering: The coil is extruded by an extrusion roller, and the pressure of the extrusion roller is 2T.

[0069] (7) Bonding: Bond the obtained film onto the PET film.

[0070] The graphene thermally conductive film of the graphene thermally conductive film coil of this embodiment has a thickness of 50 μm, a width of 150±5 mm, a length of 100-110 m, a thermal conductivity of 1300 W / mk, and a smooth film surface without bubbling or cracking.

[0071] Example 4

[0072] It is basically the same as Example 2, except that:

[0073] Step (1): the solid content of the solution is 7%, and the coating wet film thickness is 5.0 mm;

[0074] Step (3): The tightness of the diaphragm is 80%.

[0075] The graphene thermally conductive film of the graphene thermally conductive film coil of the present embodiment has a thickness of 80 μm, a thermal conductivity of 1200 W / mk, and a smooth appearance of the film surface without bubbling or cracking.

[0076] Example 5

[0077] It is basically the same as Example 2, except that:

[0078] Step (1): the solid content of the solution is 8%, and the coating wet film thickness is 6.0 mm;

[0079] Step (3): The tightness of the diaphragm is 100%.

[0080] The graphene thermally conductive film of the graphene thermally conductive film coil of the present embodiment has a thickness of 100 μm, a width of 150±5 mm, a length of 100-110 m, a thermal conductivity of 1400 W / mk, and a smooth film surface without bubbling or cracking.

[0081] Comparative Example 1

[0082] The method is basically the same as Example 2, except that: the step (4) is to place the wound coil in a gradient heating program for heat treatment, and the gradient heating temperature is: heating from room temperature to 80°C for 1 hour, then maintaining at 200°C for 60 hours and 300°C for 12 hours.

[0083] The graphene film sheet of the graphene thermal conductive film coil in this comparative example exploded.

[0084] Comparative Example 2

[0085] It is basically the same as Example 2, except that the tightness is adjusted to 20%.

[0086] The graphene film sheet of the graphene thermal conductive film coil in this comparative example exploded.

[0087] Comparative Example 3

[0088] The method is basically the same as Example 1, except that: the step (5) is to place the pretreated membrane into a graphite furnace and introduce argon gas for high-temperature firing, and the temperature curve is set as: heating from room temperature to 1000°C for 8 hours; maintaining at 1000°C for 6 hours; and maintaining at 3000°C for 15 hours.

[0089] The thermal conductivity of the graphene thermally conductive film of the graphene thermally conductive film coil of this comparative example is 1000 W / mk, and the film surface has a smooth appearance without bubbling or cracking.

[0090] Performance test results:

[0091] 1. SEM results: attached Figure 1-2 This is a scanning electron microscope image of the coil of Example 1. It can be seen from the image that the coil has a clear layered structure, excellent stacking properties, and a smoother film surface, which helps to improve the thermal conductivity. Figure 3-4 This is a scanning electron microscope image of the coil of Example 1. It can be seen from the figure that the stacking structure of the thermal conductive film in the coil is very poor and cannot form a good separation structure. In addition, there are cracks on the surface of the film, indicating that the gradient heating program in step (4) has a significant impact on whether the thermal conductive film coil can be successfully prepared and the thermal conductivity of the thermal conductive film.

[0092] 2. Thermogravimetric curve: attached Figure 5 and 6 These are the thermogravimetric curves of the thermally conductive films of Example 1 and Example 3, respectively. By comparison, it can be seen that the thermally conductive films prepared by the methods of the embodiments of the present application have stable performance, among which the stability of Example 1 is better.

Claims

1. A method for preparing a graphene thermally conductive film coil, characterized in that: The preparation method comprises the following steps in sequence: graphene oxide film preparation, striping, winding, pretreatment, graphitization, calendering, and lamination; The pretreatment step is: placing the coiled material in a gradient heating program for heat treatment; the gradient heating temperature is 25-350° C., and the treatment time is 30-120 hours.

2. The preparation method according to claim 1, characterized in that: The gradient heating temperature is: 75-85°C for 3-25h, 90-120°C for 3-25h, 130-170°C for 3-25h, 180-220°C for 3-25h, 230-270°C for 3-25h, and 280-330°C for 3-25h.

3. The preparation method according to claim 1, characterized in that: The gradient heating temperature is: heating from room temperature to 80°C for 0.5-1.5h, then maintaining at 80°C for 4-22h, 90-110°C for 4-22h, 140-160°C for 4-22h, 190-210°C for 4-22h, 240-260°C for 4-22h, and 290-310°C for 4-22h.

4. The preparation method according to claim 1, characterized in that: The gradient heating temperature is: heating from room temperature to 80°C for 1 hour, then maintaining at 80°C for 5-20 hours, 100°C for 5-20 hours, 150°C for 5-20 hours, 200°C for 5-20 hours, 250°C for 5-20 hours, and 300°C for 5-20 hours.

5. The preparation method according to claim 1, characterized in that: The temperature of the graphitization treatment step is 1000-3500° C., and the firing time is 5-40 hours.

6. The preparation method according to claim 1, characterized in that: The graphitization treatment steps are as follows: the pretreated membrane is placed in a graphite furnace and a protective gas is introduced for high-temperature firing, and the temperature curve is set as follows: heating from room temperature to 1000°C for 6-15 hours; maintaining at 1000-1500°C for 2-10 hours; maintaining at 1500-2000°C for 3-10 hours; maintaining at 2000-3000°C for 3-10 hours; and finally maintaining at 3000-3500°C for 1-4 hours.

7. The preparation method according to claim 1, characterized in that: The graphitization treatment steps are as follows: the pretreated membrane is placed in a graphite furnace and a protective gas is introduced for high-temperature firing, and the temperature curve is set as follows: heating from room temperature to 1000°C for 8-11 hours; maintaining at 1000-1500°C for 4-6 hours; maintaining at 1500-2000°C for 5-8 hours; maintaining at 2000-3000°C for 3-5 hours; and finally maintaining at 3000-3500°C for 1-3 hours.

8. The preparation method according to claim 1, characterized in that: The calendering step uses an extrusion roller to extrude the coil, and the pressure of the extrusion roller is 2-5T.

9. The preparation method according to any one of claims 2 to 7, characterized in that: The winding step of the graphene oxide is as follows: placing the graphene oxide film on a reel and a graphite tube core on a reel, and evenly winding the film onto the graphite tube core by rotating the reel and the reel, and controlling the film tightness to be 10-100%; the calculation formula of the tightness is: tightness=[film length×film thickness] / [large roll area-tube core area].

10. The graphene thermally conductive film coil prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The thickness of the graphene thermal conductive film is 5-200 μm.

Citation Information

Patent Citations

  • High-thermal-conductivity graphite film and preparation process thereof

    CN109205610A

  • High-thermal-conductivity graphene heat dissipation film and preparation method thereof

    CN112608565A

  • Graphene film and preparation method thereof

    CN113480312A

  • Preparation method of continuous graphene heat-conducting film

    CN113800504A

  • Manufacturing process of graphene heat dissipation film coiled material

    CN114590803A

Cited By

  • Preparation method of reduced graphene oxide long coiled material

    CN120573690A